    Influence of Shim Layers on Progressive Failure of a Composite Component in Composite-Aluminum Bolted Joint in Aerospace Structural Assembly

    2018-03-29 07:36:09,*,,

    ,*,,

    1.Department of Aerospace Manufacturing Engineering,Jiangsu Key Laboratory of Precision and Micro-Manufacturing Technology,Nanjing University of Aeronautics and Astronautics,Nanjing 210016,P.R.China;

    2.AVIC Xi′an Aircraft Industry(Group)Company LTD,Xi′an 710089,P.R.China

    0 Introduction

    Due to their high specific stiffness,higher specific strength and other better performances,composite materials are hugely being utilized in the aerospace industries for both civil and military applications[1,2].Although composite materials are extensively being used because of the aforementioned reasons,composite structures are susceptible to damage as a result of their brittle nature and other technical issues like shimming[3,4].Aluminum alloys,however,are still being used in the aerospace industry despite the growing usage of composite materials.An example of the use of hybrid materials (that is composite-metal structures)is the fighter jet JAS39Gripenas shown in Fig.1[5].Furthermore,some aircraft manufacturers like Airbus still maintain a significant percentage of aluminum alloys in its manufactured aircrafts(A320′s airframe is composed of aluminum alloy)which make the assembly of hybrid structures(composite-aluminum)inevitable.In the assembly of aerospace structural components,there are several mechanical fasteners employed and as a result,holes have to be drilled for the installation of these mechanical fasteners.Before starting to drill the hole and with subsequent fastener installation,it is imperative to check all joints for the presence of gaps.This is because the presence of gaps can needlessly preload the metallic members when fasteners are installed prompting a condition that can cause premature fatigue cracking and even stress corrosion cracking of an aluminum component.Howbeit,gaps in structures containing composites can cause even more serious problems than in metallic structures.Since composites do not yield and are more brittle and less lenient than metals,excessive gaps can result in delaminations when they are pulled out during fastener installation.

    Fig.1 Composite and metal materials in JAS39Gripen

    This phenomenon put the composite in a bending due to the exerted force by the fastener drawing the parts together and can develop matrix cracks and/or delaminations around the holes.Cracks and delaminations normally occur in multiple layers through the thickness and can significantly affect the joint strength[6].

    There have been several studies into the progressive failure of composite materials.Tsai and Wu[7]; Reddy and Pandey[8]; Turvey[9];and Hashin[10]revolutionized the studies into the progressive failures of composite materials.Other authors like Chang and Chang[11]developed the progressive damage analysis of notched laminated composites subjected to tensile loading.The progressive failure method employed in Ref.[11]was a nonlinear FEA that used the modified Newton-Raphson iteration technique to develop the state of stresses in a composite component.Also,Chang and Lessard[12]conducted an investigation into the damage in laminated composites containing an open hole subjected to a compressive loading.Contributing to the advances in failure theories of composite materials,Reddy et al.[13]evaluated both linear and non-linear first-ply failure loads of composite plates for different edge conditions and load cases.The apparent complexities associated with composite materials made the aforementioned failure theories to have had limitations which necessitated and motivated other authors to further refine these existing theories.An example of a refined theory for the progressive failure analysis of composite materials has been developed and successfully implemented in the works of Ref.[14].

    There has been some published literature on shimming[15-17],but most studies were skewed toward liquid shims[18-22].With regard to the analysis of failure of composite materials with ashim,the authors Hühne et al.[18];Dho^te et al.[19];Comer et al.[20];and Liu[22]conducted studies using single-lap bolted joints with a liquid shim.In investigations of Ref.[22],in particular,it was concluded that the stiffness of the joints decreased due to the presence of liquid shim,and the joint stiffness decreased with an increasing liquid shim thickness.Comer et al.[20]investigated thermomechanical fatigue tests on hybrid joints with liquid shim layers and concluded that there was no degradation in respect to the mechanical stiffness for the liquid shim.Zhai et al.[23]studied the effect of solid shim and liquid shim on compositealuminum bolted joints by using a 3DDigital Image Correlation.Although,the investigation of Ref.[23]was″supposed″to be about solid shim and liquid shim,however,it was carried out ex-perimentally hence the objective of this research to investigate the influence of both liquid and solid peelable fiberglass shim using finite element analysis and experimental study.

    1 Materials for Experimental Testing and Finite Element Modeling of Composite-Aluminum Bolted Joint

    The 3Dfinite element(FE)assembled model and the test specimens were an idealization of an aircraft′s wingbox sub-structural components.That is a composite wing panel and an aluminum rib.Aluminum alloy 7075-T651was chosen for this study because of its use in the aerospace industry for highly stressed and critical structural parts[6,7].The test specimens,as well as the FE model,were composed of the parts(Figs.2,3):A hi-shear corporation fastener with a protruding head(HST-12-8)and a washer all composed of aerospace grade titanium alloy (Ti-6Al-4VSTA);one plate made of the carbon fiber-reinforced polymer (CFRP) material-carbon-epoxy IMS-977-2(Cytec Industries Inc.)with the quasiisotropic stacking sequence being[+45/90/-45/0/90/0/-45/90/+45/-45]sand with a total ply thickness of 0.188mm for 20plies;the other plate is made of a high strength aerospace grade aluminum alloy,7075T651.Two CFRP support plates were adhesively bonded to the main plates to avoid excessive bending.Commercially available liquid shim material-Hysol EA9394of Henkel Corporation and a solid peelable fiberglass of LAMECO group manufactured under the COMAC standard CMS-MT-301were the other materials utilized.The FE model and the test specimens were based on the test standards of American Society for Testing and Materials(ASTM),D5961/D5961M-13[24]and recommendations in Ref.[20].The single-lap model of the composite-aluminum bolted joint specimen is shown in Figs.2,3.

    Fig.2 Dimensions in millimeter of the single-lap

    Fig.3 Dimensions in millimeter of the single-lap composite-composite-aluminum bolted joint without shim aluminum bolted joint with shim

    2 Finite Element Model

    A non-linear 3Dsolid elements model of a single-lap composite-aluminum assembled structure with and without shim layers under a quasistatic tensile loading was developed using the commercial FE program ABAQUS/Standard 6.13[25]and in accordance with Refs.[20,24].The developed model was without the doublers as shown in Fig.4.The bolt,collar,and the washer were modeled as a unit as shown in Fig.5because they were engaged together and they are composed of the same titanium material.There were nine different kinds of composite-aluminum bolted joints.Namely,without a shim,with a liquid shim (0.3,0.5,0.7and 0.9mm thickness)and with solid peelable fiberglass(0.3,0.5,0.7and 0.9mm thickness).

    The strength and elastic properties[26]for the carbon-epoxy IMS-977-2substrate are shown in Table 1.The meshed CFRP had a total number of 37 040elements after it has been seeded with 20 elements in the thickness direction,15elements equally distributed in the area covered by the fastener head and 20elements equally distributed on the half periphery of each fastener hole along the circumferential direction.Structured hexagonal mesh controls were assigned and a stack direction assigned in the isometric view.The meshed CFRP plate as shown in Fig.6was developed using the element type C3D8R:An eight-node linear brick,reduced integration,hourglass control in Abaqus.

    Fig.4 Developed model

    Fig.5 FE model of bolt-collar-washer

    Table 1 CFRP elastic and strength properties

    Fig.6 CFRP meshed FE model

    The aluminum plate and titanium parts were modeled using their elasto-plastic material behaviors as shown in Table 2.The AA7075-T651was modeled same as the CFRP with the only differences being the seeding in the thickness direction where 10elements were used and there was no assigning of stacking direction.The meshed AA7075-T651plate in Fig.7has a total number of 17 520elements.Titanium parts(meshed Ti-6Al-4VSTA is shown in Fig.8)were modeled same as the CFRP but with different approximate global size(0.6used)and mesh controls(sweep used).

    Fig.7 AA7075-T651meshed FE model

    The Hysol EA9394of Henkel Corporation and the solid peelable fiberglass were modeled using their elastic properties as shown in Table 3.The shim materials(an example shown in Fig.9is a meshed model of a shim with a thickness of 0.3mm)were also modeled same as the CFRP but with an approximate global size of 0.7and seeded with 3elements in the thickness direction for a shim thickness of 0.3mm (5elements and 7elements for shim thickness of 0.5mm and 0.7mm,respectively).

    Fig.8 Bolt-collar-washer meshed FE model

    Fig.9 Shim material meshed FE model

    Table 2 Elasto-plastic properties of AA7075-T651[27]and Ti-6Al-4VSTA[14]

    Table 3 Elastic properties of Hysol EA9394[28]and solid peelable fiberglass[29]

    The boundary conditions of the FE model in Fig.10has the″Reference Node 2″(RP-2)which is the aluminum plate held fixed in all six degrees of freedom (Ux,Uy,Uz,Rx,RyandRz)because it is clamped and the″Reference Node 1″(RP-1)which is the CFRP plate held fixed in two translational directions(UyandUz)and in all three rotational directions(Rx,RyandRz).A pull distance of 10mm was then applied to RP-1in theUxdirection.

    Fig.10 Boundary conditions on the plates

    Fig.11 Bolt load application

    The clamping force of 10kN[30]produced by the tightening torque was applied through a bolt load function as shown in Fig.11in ABAQUS.The contact relationships were defined for contact pairs interacting with each other using a stringent master-to-slave rule[25].A total of six contact pairs were defined and implemented in the FE model under the interaction section in Abaqus.Contact was modeled between (a)the main plates,(b)between fastener(shanks)and plate holes,(c)between shim,plates,fastener shanks and plate holes,(d)between aluminum plate and washer(bottom surface)and(e)between collar(upper surface)and composite plate.The contacts were defined using the penalty method with hard contact,friction,and finite sliding.″Finite-Sliding″allows for any arbitrary motions of the faying surfaces and the active contact constraints any changes during the analysis.″Small-Sliding″is used if there is a relatively little sliding of any surfaces interacting with each other.A surface-tosurface contact option was used for all contacts,several coefficients of friction were used in the model and their value depended on the components in contact.The frictional coefficient for the interaction between the composite plate and the titanium parts:0.16[30].Frictional coefficients of 0.288[31]and 0.235[32]were used for interactions between aluminum plate and titanium parts,and between composite plate and aluminum plate,respectively.The additional frictional coefficient which is 0.2(assumed),was assigned to all other parts interacting with the shim materials.The surface of the modeled shim was tied onto the composite plate and as shown in Fig.12,special elements(springs/dashpots)were used to connect points to ground.RP-1was used to create a set(set-coupling)and with set-coupling as the control points,a constraint(coupling kinematictype)was created using the surface on which RP-1was situated.

    With this done,the set-coupling was used to generate the needed FEA results for analysis.

    Fig.12 Boundary conditions on the assembled model

    3 Progressive Damage Modeling of CFRP

    Damage in composite structures is internally initiated and accumulated over a period of time before structural failure.The use of failure criteria alone to predict the ultimate failure is not enough because the failure criteria predict the onset of the damage occurring hence there is the need to develop an algorithm to simulate the nonlinear material behavior in the composite structure.The developed algorithm:The progressive damage,is based on the ply-discount method.The failure modes with their criterion;and the material property degradation rules used in the progressive damage model(PDM)are adequately documented in Ref.[14].The PDM is an integration of the stress analysis,failure analysis,and material property degradation.The flowchart for the progressive failure algorithm[33]is shown in Fig.13and the following steps give a detailed explanation of the flowchart:

    Step 1The development of the 3Dsolid FE model of the composite-aluminum bolted structure by inputting the various material properties,boundary conditions,contacts,initial load and final load step.

    Step 2Non-linear stress analysis is performed.

    Step 3Failure analysis is performed by applying the failure criteria.

    Step 4Ply failures are checked:

    (1)If no failure is predicted,the applied load,F(xiàn)mis increased by an increment,ΔFaccording to the equation:Fm=Fm=1+ΔF,and the program goes back to Step 2.

    (2)If there is a mode of failure being predicted,then the program moves on to the next step.

    Step 5The degradation of the material properties of the plies that had failed.

    Step 6Final failure checking:

    (1)If the final failure is reached,the program stops.

    (2)If not,the program goes back to Step 2 and the non-linear stress analysis is carried out again so as to calculate the redistributed stresses.Convergence at a load step is assumed(is proved to be a good compromise between accuracy and time consumption)[34]when no additional failure is detected.

    The PDM written in FORTRAN was implemented into Abaqus/Standard as a user-defined subroutine,USDFLD.The degradation rules were implemented using the field variables(FV)which are dependent on the failure criterion of each failure mode.The USDFLD, within ABAQUS,provides the user a method to write a program that updates the FV at every integration point for each increment in the analysis according to the failure criteria values obtained during the solution.

    At the beginning of each increment,the USDFLD,using the utility subroutine GETVRM,accesses the material point quantities for every integration point in the model and these solutiondependent field variables(SDV)are then used to create an array of FVs to define the material properties of the next iteration[34].Additional,solution-dependent state variables (STATEV),which provide a dependence of each material point on its history,may be updated in this subroutine and the updated values are then passed to another user subroutines that are called at the material point.These state variables are eventually transferred back into the main Abaqus program.According to the different failure modes,there are four different state variables which are defined to display the progression of damage during the post-processing.The failure modes simulated are matrix failure(FV1),fiber failure(FV2),fibermatrix shear failure(FV3)and shear non-linearity(FV4).After the stress analysis,the generated stress values are then used to compute the failure criterion values.If any of the values are greater or equal to 1,the related field variable for the integration point with the highest failure criterion value is set permanently to 1,which indicates failure(it is important to note that the degradation models implemented within ABAQUS degrade at the integration points rather than elements).And these solution-dependent field variables are then used to define the material properties of the next iteration.

    Fig.13 Flowchart of the progressive damage algorithm

    4 Experimental Work

    The test specimens consisted of two plates(composite and aluminum),shim materials(liquid shim-Hysol EA9394and solid shim-peelable fiberglass)and a prestressed titanium bolt with a protruding head.The experiment was performed under quasi-static tensile loading using an electronic universal testing machine (SANS 4105).The test machine was manufactured in accordance with the GB/T 228-2002code of Chinese National Standards.The tests were conducted at a loading velocity of 10mm/s at room temperature.

    4.1 Test specimen preparation

    The specimen in Fig.14was prepared in accordance with the configurations in Refs.[20,24].The liquid shim was prepared in accordance with the manufacturer′s instructions and applied to the composite plate.The prepared specimens were clamped and allowed at least four days to cure at room temperature.Finally,the plates were fastened together by the torquing off of the collars with finger-tightening.

    Fig.14 Composite-aluminum bolted structure

    Fig.15 Test specimen with a liquid shim

    Fig.16 Test specimen with a solid shim

    For the specimen with shim materials,the shim adhered to the mating surface of the composite plate,as shown in Figs.15,16,for a specimen with a liquid shim and a solid shim,respectively.The specimen without any shim is also shown in Fig.17.

    Fig.17 Test specimen without shim

    4.2 Test set-up and procedure

    The test specimens were rigidly clamped into the testing machine as shown in Fig.18.The load application was carried out with a constant traverse speed until structural collapse occurred.

    Fig.18 Test specimen rigidly clamped into the testing machine

    The force against the displacement of the specimens was recorded by a computer.Fig.1 9 shows the experimental arrangement.

    Fig.19 Test set-up for the experiment

    The experiments were stopped after the load had dropped to 15%of its peak load or after the occurrence of an excessive displacement.Each test configuration was repeated with three test specimens and the results that corresponded accurately with the FE results has been presented in this paper.

    5 Results and Discussion

    The numerically simulated results were compared with the experimental data and they were in agreement very well with each other.Subsequently discussed are the load-displacement behavior and the influence of the shim layers on the damage behavior of the composite component.The test results are shown in Figs.20(a—e)and Figs.21(a—e).

    5.1 Load-displacement evaluation

    The numerically simulated load-displacement behavior of the composite component was very similar with the experimentally determined data.Figs.20(a—e)show the load-displacement curves for specimen without shims,0.3,0.5,0.7and 0.9 mm shim thickness,respectively(both liquid and solid shim).

    The maximum experimentally determined load for a specimen without any shims was 16.09 kN at a displacement of 6.1mm but the maximum experimentally determined load for a specimen with a 0.3mm liquid shim thickness was 19.83kN at a displacement of 9.7mm.And also,the maximum experimentally determined load for a specimen with a 0.3mm solid shim thickness was 18.60kN at a displacement of 7.9mm.This kind of trend where all the maximum experimentally determined loads and displacements for specimens with shims being higher than the maximum experimentally determined loads and displacements for specimen without any shims is also obviously seen in Fig.20.The reason for such an observation is the presence of shim.The presence of shims increased the amount of load needed for failure and also increased the strength of the component by increasing the displacement at which failure occurs.

    A further examination of the test results reveals that,with regard to the load-displacement evaluation,the simulated load values were higher than the experimentally determined load values at the same displacement and the differences in these values could be as a result of several factors but predominately,it could be the:(1)Differences in material properties used in the FE modeling and the″actual properties″of the test specimen;(2)Inherent limitations of the failure method used to simulate the damage;and(3)Degradation rules being somewhat different from the″actual failure progression″of the test specimen.

    The progression of the load-displacement curves for the simulated conditions and the experimental conditions were as a result of friction so,the choice of the frictional coefficient to be used for modeling is very important.It has been observed that there is a linearity in the behavior of the composite component initially before reaching the peak loads and subsequently experiencing large displacements before failure.The progressive damage causes such a non-linear curve pattern until the ultimate load was reached.However,the ultimate load identified in the experiments could not be achieved exactly numerically.In comparison,the specimens with liquid shim series were a better fit for gap thickness of 0.3,0.5,0.7mm whereas specimens with solid shim series were better situated for the gap thickness of 0.9mm.

    5.2 Influence of shim layer

    Fig.20 Load-displacement trends for specimens without shim and with different shim thicknesses

    Fig.21 Stiffness-load trends for specimens without shim and with different shim thicknesses

    To be able to estimate the influence of the shim layers on the damage of the composite component,it is imperative to plot the stiffness-load curves.Figs.21 (a—e)show the stiffness-load curves for specimen without shims,with 0.3,0.5,0.7,0.9mm (both liquid and solid shim)shim thickness,respectively.As shown in Figs.21(a—d),generally,the stiffness for both the experiment and that of the numerical simulation decreased with an increasing load up to the failure point of the component before gradually also decreasing with a decreasing load.As for Fig.21(e),the stiffness for both the experiment and that of the numerical simulation decreased with an increasing load up to the failure point of the component before gradually also decreasing with a decreasing load for the liquid shim specimen but for the solid shim specimen,the stiffness gradually increased with an increasing load up to about a displacement of 2.0mm before eventually decreasing with an increasing load up to the component′s failure point and then finally decreased with a decreasing load.Probing further the curves in Fig.20,it was obvious that with regard to the stiffness-load evaluation,the simulated stiffness values were higher than the experimentally determined stiffness values and it is much significantly higher for the about first six stiffness values.The differences in these values could be as a result of the factors discussed in Section 5.1.

    The variations observed in Figs.21(a—e)are predominately due to the dissipation of friction which magnifies the fact that the choice of the coefficient of friction for the FE modeling is important.Afterward,the damage evolution starts and the linear stiffness decreases yield meant that some elements were completely damaged while others still had some stiffness in them.The specimen without any shim material generally exhibited higher stiffness than all liquid shim series(with the exception of 0.9mm shim thickness)and all solid shim series(with the exception of 0.3mm shim thickness and 0.5mm shim thickness).

    It is also clear from Figs.21(a—e)that,the use of liquid shim generally caused a reduction in the joint stiffness for 0.3,0.5,0.7mm shim thickness.It is worth noticing that the solid shim was a better fit for the 0.9mm shim thickness because it considerably gave a better stiffness degradation performance and this may be as a result of the higher tensile modulus of the solid peelable fiberglass shim.Fig.22shows the damaged specimens after the experiments.

    Fig.22 Damaged specimens

    To demonstrate the″somewhat limitations″of the PDM used in simulating the damages,a closer look was taken at the damages for the test specimen without any shim material and the 0.3 mm shim thickness(both liquid and solid shim)as an illustration.The damages for the test specimen without any shim material and the 0.3mm shim thickness(both liquid and solid shim)are shown in Figs.23(a—c),respectively.

    Fig.23 Damaged specimens without shim and with liquid and solid shims

    In the numerical simulation,the failure modes matrix failure,fiber failure as well as the fiber-matrix failure could be displayed but the shear non-linearity could not be″adequately″displayed because the FE-model is an idealization of the reality hence some assumptions were made.Those assumptions definitely had an effect on the actual damage.The view taken for the simulated damaged images is shown in Fig.24.

    Fig.24 View used for taking FV1,F(xiàn)V2,F(xiàn)V3and FV4 damages

    Fig.25 FV1damage for specimens without shim and with liquid and solid shim thicknesses

    Fig.26 FV2damages for specimens without shim and with liquid and solid shim thicknesses

    Figs.25(a—c),F(xiàn)igs.26 (a—c),F(xiàn)igs.27(a—c)and Figs.2 8(a—c)show the simulated four damages(FV1,F(xiàn)V2,F(xiàn)V3,and FV4,respectively)for the specimen with no shim material,with a 0.3mm liquid shim thickness,and with a 0.3mm solid shim thickness.

    In addition to an earlier explanation as to why the shear non-linearity damages in Figs.28(a—c)could not be″adequately″ displayed,it should be noted that it has been assumed in the theory being used in simulating the shear non-linearity that,the non-linearity mainly was caused by the micro-cracking in the matrix and the PDM could not simulate″such microcracking″.

    6 Conclusions

    Fig.27 FV3damages for specimens without shim andwith liquid and solid shim thicknesses

    A three-dimensional finite element model of a single-lap,single-bolt composite-aluminum assembled structure has been developed to investigate the influence of varying shim layers on the progressive damage/failure of a composite component in a bolted composite-aluminum aerospace structural assembly and the numerical results validated against the experimental results were generally in good agreement.From the analysis,the following was discovered:

    (1)The shimming procedure as agreed upon by the aerospace industry for the resolution of assembly gaps in bolted joints for composite materials is same as that for a composite-aluminum structure:liquid shim series prolonged the service life of the composite component for the assembly gaps of 0.3,0.5and 0.7mm;and a solid peelable fiberglass shim most had a better influence on the 0.9mm assembly gap.

    (2)The shim layers considerably influenced the structural strength of the composite component by delaying its failure,thereby increasing its service life.

    Fig.28 FV4damages for specimens without shim and with liquid and solid shim thicknesses

    (3)Increasing the shim layer′s thickness led to a significant corresponding effect on the stiffness but with minimal effect on the ultimate load.

    The aforementioned observations cannot be definitive because other factors,such as thermal expansion coefficients,failure, and fracture mechanisms,and degree of plasticity,might influence the trend observed in this paper for a composite-aluminum structure.

    Acknowledgements

    The authors wish to acknowledge the Innovation Foundation of National Research Center for Commercial Aircraft Manufacturing Engineering Technology in China (No.SAMC13-JS-13-021)and Jiangsu Key Laboratory of Precision and Micro-Manufacturing Technology for the provision of financial support.

    [1] MALLICK P K.Fiber-reinforced composites:Mate-rials,manufacturing,and design[M].3rd Edition.New York:CRC Press,2007:1-12.

    [2] LAURIN F,CARRERE N,MAIRE J F.Strength analysis methods for high stress gradient parts in composite structures ensuring design office requirements[J].Proc IMechE,Part G:J Aerospace Engineering,2011,225(3):291-301.

    [3] WALKER K.EASA widens AD for A380cracks;Boeing confirms 787shims[EB/OL].[2012-02 08]/(2016-10-18).http://atwonline.com/aircraft-ampengines/easa-widens-ad-a380-cracks-boeing-confirms-787-shims.

    [4] FALZON B.The airbus A380wing cracks:an engineer′s perspective [EB/OL].http://the conversation.com/the-airbus-a380-wing-cracks-an-engineersperspective-5318.[2012-2-10](2016-10-18).

    [5] KAPIDZIC Z.Strength analysis and modeling of hybrid composite-aluminum aircraft structures [D].Link ping:Link ping University,2013:3.

    [6] CAMPBELL F C.Manufacturing technology for aerospace structural materials[M].1st Edition.Oxford:Elsevier Science and Technology,2006:498-499.

    [7] TSAI S W,WU E M.A general theory of strength for anisotropic materials[J].J Comp Mater,1971,5(1):58-80.

    [8] REDDY J N,PANDEY A K.A first ply failure analysis of composite laminates[J].Computers Struct,1987,25(3):371-393.

    [9] TURVEY G V.An initial flexural failure analysis of symmetrically laminated cross-ply rectangular plates[J].Int J Solids Struct,1980,16(5):451-463.

    [10]HASHIN Z.Analysis of cracked laminates:A variationalapproach[J].Mech Mater,1985,4(2):121-136.

    [11]CHANG F K,CHANG K Y.A progressive damage model for laminated composites containing stress concentrations[J].J Comp Mater,1987,21(9):834-855.

    [12]CHANG F K,LESSARD L B.Damage tolerance of laminated composites containing an open hole and subjected to compressive loadings:Part I—Analysis[J].J Comp Mater,1991,25(1):2-43.

    [13]REDDY Y N S,REDDY J N.Linear and non-linear failure analysis of composite laminates with transverse shear[J].Compos Sci Tech,1992,44(3):227-255.

    [14]KAPIDZIC Z,NILSSON L,ANSELL H.Finite element modeling of mechanically fastened composite-aluminum joints in aircraft structures[J].Compos Struct,2014,109:198-210.

    [15]SMITH J.Concept development of an automated shim cell for F-35forward fuselage outer mold line control[D].Menomonie:University of Wisconsin-Stout,2011.

    [16]LEE R.Evaluation of shimming options with applications to JSF [EB/OL].[1999-12]/(2016-11-21).http:∥ materialchemistry.com/DreamHC/Download/JSF%20Shimming%20Analysis.pdf.

    [17]CARACCIOLO P,KUHLMANN G. Reliability analysis in bolted composite joints with shimming material[C]∥25th international congress of the aeronautical sciences.Hamburg,Germany,2006:524.

    [18]H HNE C,ZERBST A K,KUHLMANN G,et al.Progressive damage analysis of composite bolted joints with liquid shim layers using constant and continuous degradation models [J].ComposStruct,2010,92(2):189-200.

    [19]DH TE J X,COMER A J,STANLEY W F,et al.Study of the effect of liquid shim on single-lap joint using 3Ddigital image correlation[J].ComposStruct,2013,96:216-225.

    [20]COMER A J,DH TE J X,STANLEY W F,et al.Thermo-mechanical fatigue analysis of liquid shim in mechanically fastened hybrid joints for aerospace applications[J].Compos Struct,2012,94(7):2181-2187.

    [21]DH TE J X,COMER A J,STANLEY W F,et al.Investigation into compressive properties of liquid shim for aerospace bolted joints[J].Compos Struct,2014,109:224-230.

    [22]LIU L.The influence of the substrate′s stiffness on the liquid shim effect in composite to titanium hybrid bolted joints[J].Proc IMechE,Part G:J Aerospace Engineering,2014,228(3):470-479.

    [23]ZHAI Y,LI D,LI X,et al.An experimental study on the effect of joining interface condition on bearing response of single-lap,countersunk composite-aluminum bolted joints[J].Compos Struct,2015,134:190-198.

    [24]ASTM Standard D5961/D 5961M-13.Standard test method for bearing response of polymer matrix composite laminates[S].West Conshohocken,PA,USA:ASTM International,2013.

    [25]ABAQUS.Inc.ABAQUS version 6.13Documentation[M].Velizy-Villacoublay:Dassault Systemes/SIMULIA,2013.

    [26]de LUCA,CAPUTO F,LAMANNA G,et al.Study of analytical models for predicting impact damage to composite structures[C]∥Italian Association for Stress Analysis 42nd National Congress.Salerno,Italy:University of Salerno,2013:11-14.(in Italian)

    [27]ZHAO T W,JIANG Y.Fatigue of 7075-T651aluminum alloy[J].Int J Fatigue,2008,30(5):834-849.

    [28]SUN C T.Adhesively bonded joints,Part 1:bondline thickness effects and hybrid design of adhesively bonded joints[R].DOT/FAA/AR-11/1,P1,USA:FAA report,F(xiàn)ebruary 2014.

    [29]HARTMAN D R,GREENWOOD M E,MILLER D M.High Strength Glass Fibers:1-Pl-19025-A[R].Owens Corning Inc.,Technical Paper Ref.July 1996.Reprinted by AGY LLC as Pub.No.LIT-2006-111,F(xiàn)ebruary 2006.

    [30]STOCCHI C,ROBINSON P,PINHO S T.A detailed finite element investigation of composite bolted joints with countersunk fasteners[J].Compos Struct:Part A,2013,52:143-150.

    [31]CHAKHERLOU T N,OSKOUEI R H,VOGWELL J.Experimental and numerical investigation of the effect of clamping force on the fatigue behaviour of bolted plates[J].Eng Fail Anal,2008,15(5):563-574.

    [32]EKH J,SCHON J,MELIN L G.Secondary bending in multi fastener,composite-to-aluminium single shear lap joints[J].Compos Struct:Part B,2005,36(3):195-208.

    [33]TSERPES K I,PAPANIKO P,KERMANIDIS T H.A three-dimensional progressive damage model for bolted joints in composite laminates subjected to tensile loading[J].Fat Fract Engng Mater Struct,2001,24:663-675.

    [34]LIU L,ZHANG J,CHEN K,et al.Combined and interactive effects of interference fit and preloads on composite joints[J].Chin J Aero,2014,27(3):716-729.

    一二三四在线观看免费中文在| 精品久久久久久成人av| 午夜福利在线在线| 99在线视频只有这里精品首页| 熟女电影av网| 亚洲av熟女| 搞女人的毛片| 中文字幕高清在线视频| 国产一区二区在线av高清观看| 国产探花在线观看一区二区| 亚洲精品色激情综合| 最新美女视频免费是黄的| 国产精品久久久av美女十八| 最新在线观看一区二区三区| 国产99白浆流出| 一级片免费观看大全| 日韩国内少妇激情av| 两个人视频免费观看高清| 欧美绝顶高潮抽搐喷水| 欧美性猛交╳xxx乱大交人| 成人一区二区视频在线观看| 五月玫瑰六月丁香| 99精品在免费线老司机午夜| 国产av不卡久久| 免费在线观看日本一区| 欧美极品一区二区三区四区| 最近在线观看免费完整版| 长腿黑丝高跟| av中文乱码字幕在线| 欧美精品亚洲一区二区| 欧洲精品卡2卡3卡4卡5卡区| 88av欧美| 在线观看舔阴道视频| 久久中文字幕一级| 天天一区二区日本电影三级| 99久久无色码亚洲精品果冻| 在线a可以看的网站| 久久午夜亚洲精品久久| 亚洲av成人不卡在线观看播放网| 中出人妻视频一区二区| 成人18禁在线播放| 别揉我奶头~嗯~啊~动态视频| 91av网站免费观看| 男女做爰动态图高潮gif福利片| 999精品在线视频| 国产精品1区2区在线观看.| 国产成人aa在线观看| 国产又色又爽无遮挡免费看| 黑人欧美特级aaaaaa片| 欧美日韩中文字幕国产精品一区二区三区| 欧美日韩国产亚洲二区| 最近最新免费中文字幕在线| 一边摸一边做爽爽视频免费| 久99久视频精品免费| 国产在线观看jvid| 国产又黄又爽又无遮挡在线| 女生性感内裤真人,穿戴方法视频| 亚洲成av人片在线播放无| 免费搜索国产男女视频| 999久久久精品免费观看国产| 国产日本99.免费观看| 亚洲精品久久成人aⅴ小说| 夜夜躁狠狠躁天天躁| 精品国产乱码久久久久久男人| 免费无遮挡裸体视频| 麻豆成人午夜福利视频| 少妇人妻一区二区三区视频| 亚洲欧洲精品一区二区精品久久久| 床上黄色一级片| 国产精品国产高清国产av| 欧美色视频一区免费| 国产亚洲精品第一综合不卡| 久久久久精品国产欧美久久久| 亚洲精品国产精品久久久不卡| 成人高潮视频无遮挡免费网站| 桃红色精品国产亚洲av| 女人高潮潮喷娇喘18禁视频| 丰满人妻熟妇乱又伦精品不卡| 欧美一区二区国产精品久久精品 | a在线观看视频网站| 99国产极品粉嫩在线观看| 久久伊人香网站| 国产一区二区在线av高清观看| 色老头精品视频在线观看| 欧美日韩一级在线毛片| 亚洲国产看品久久| 亚洲 欧美一区二区三区| 国产成人精品无人区| 久久久久久九九精品二区国产 | 国产精品1区2区在线观看.| 91成年电影在线观看| 黄色丝袜av网址大全| 中文字幕熟女人妻在线| 亚洲欧美精品综合一区二区三区| 操出白浆在线播放| 黄色女人牲交| 国产av一区在线观看免费| 一个人免费在线观看的高清视频| av福利片在线观看| 夜夜夜夜夜久久久久| 波多野结衣高清作品| 白带黄色成豆腐渣| 国产成人一区二区三区免费视频网站| 久久精品国产亚洲av香蕉五月| 亚洲中文日韩欧美视频| 免费看十八禁软件| 亚洲国产精品sss在线观看| 国内精品久久久久精免费| 国产精品久久久久久人妻精品电影| 国内少妇人妻偷人精品xxx网站 | 亚洲五月婷婷丁香| 亚洲乱码一区二区免费版| 两个人看的免费小视频| 亚洲aⅴ乱码一区二区在线播放 | 日本免费a在线| 午夜免费激情av| 巨乳人妻的诱惑在线观看| 真人做人爱边吃奶动态| 成人手机av| 午夜a级毛片| 久久久久免费精品人妻一区二区| 午夜精品久久久久久毛片777| 日韩欧美一区二区三区在线观看| 国产精品一及| 丰满人妻一区二区三区视频av | 亚洲欧美一区二区三区黑人| 天天添夜夜摸| 神马国产精品三级电影在线观看 | 国产一区在线观看成人免费| 91九色精品人成在线观看| 丝袜美腿诱惑在线| 变态另类成人亚洲欧美熟女| 免费看日本二区| 亚洲狠狠婷婷综合久久图片| 亚洲成人久久性| 人妻丰满熟妇av一区二区三区| 欧美日韩一级在线毛片| 国产成人一区二区三区免费视频网站| 在线观看日韩欧美| 亚洲成av人片免费观看| 一边摸一边抽搐一进一小说| 久久精品国产亚洲av高清一级| 欧美成人性av电影在线观看| www.自偷自拍.com| 黑人操中国人逼视频| 非洲黑人性xxxx精品又粗又长| 欧美性猛交黑人性爽| 99久久久亚洲精品蜜臀av| 成年女人毛片免费观看观看9| 久久中文字幕一级| 精品久久久久久,| 亚洲专区字幕在线| 久久久国产成人精品二区| 国产视频一区二区在线看| 一卡2卡三卡四卡精品乱码亚洲| 在线观看美女被高潮喷水网站 | 18禁黄网站禁片午夜丰满| 国产欧美日韩精品亚洲av| 国产一级毛片七仙女欲春2| 两个人看的免费小视频| 亚洲精品久久国产高清桃花| 亚洲精品久久成人aⅴ小说| www日本在线高清视频| 久久草成人影院| 日日干狠狠操夜夜爽| 精华霜和精华液先用哪个| 欧美激情久久久久久爽电影| 欧美日韩亚洲国产一区二区在线观看| 国产高清有码在线观看视频 | 国产精品一区二区三区四区久久| 精品国产超薄肉色丝袜足j| 久久久精品大字幕| 一级作爱视频免费观看| 国产午夜精品久久久久久| 精品电影一区二区在线| 日日摸夜夜添夜夜添小说| 99热6这里只有精品| av在线天堂中文字幕| 欧美又色又爽又黄视频| 亚洲av成人一区二区三| 日本一区二区免费在线视频| 久久精品综合一区二区三区| 亚洲精品在线观看二区| 真人做人爱边吃奶动态| 无人区码免费观看不卡| 国产精品爽爽va在线观看网站| 婷婷精品国产亚洲av在线| 看片在线看免费视频| 亚洲免费av在线视频| 欧美成人性av电影在线观看| 草草在线视频免费看| 精品一区二区三区视频在线观看免费| 亚洲av成人精品一区久久| 在线观看免费午夜福利视频| 成在线人永久免费视频| www日本黄色视频网| 在线a可以看的网站| 怎么达到女性高潮| 99热6这里只有精品| 18禁美女被吸乳视频| 午夜a级毛片| 欧美日韩黄片免| 亚洲av片天天在线观看| 特大巨黑吊av在线直播| 十八禁人妻一区二区| 亚洲精品国产精品久久久不卡| 国产三级在线视频| av免费在线观看网站| 国内精品久久久久精免费| 精品一区二区三区四区五区乱码| 我要搜黄色片| 国产精品av视频在线免费观看| 国产午夜福利久久久久久| 亚洲av成人一区二区三| 美女扒开内裤让男人捅视频| 男插女下体视频免费在线播放| 国产一区二区在线av高清观看| 亚洲成人精品中文字幕电影| 国产黄片美女视频| 可以在线观看毛片的网站| 国产成人欧美在线观看| 1024视频免费在线观看| 久久久久久国产a免费观看| 国产精品久久久av美女十八| 亚洲人成网站在线播放欧美日韩| 精品久久久久久久久久免费视频| 很黄的视频免费| 亚洲国产精品成人综合色| 日本精品一区二区三区蜜桃| 床上黄色一级片| 成年人黄色毛片网站| 很黄的视频免费| √禁漫天堂资源中文www| 午夜精品一区二区三区免费看| 久久精品国产综合久久久| 女同久久另类99精品国产91| 国产在线精品亚洲第一网站| 成年女人毛片免费观看观看9| 亚洲欧美日韩高清专用| 国产精品av久久久久免费| 亚洲男人天堂网一区| 欧美av亚洲av综合av国产av| 国产一级毛片七仙女欲春2| 757午夜福利合集在线观看| 男女那种视频在线观看| 99久久精品国产亚洲精品| 国产成人精品久久二区二区91| 美女高潮喷水抽搐中文字幕| 午夜亚洲福利在线播放| 在线观看日韩欧美| 欧美丝袜亚洲另类 | 看黄色毛片网站| 欧美另类亚洲清纯唯美| 三级毛片av免费| 一边摸一边抽搐一进一小说| 淫秽高清视频在线观看| 色综合亚洲欧美另类图片| 三级国产精品欧美在线观看 | 国内精品久久久久久久电影| 精品久久久久久久末码| 亚洲狠狠婷婷综合久久图片| 久久中文看片网| 国产野战对白在线观看| 成人特级黄色片久久久久久久| 老司机深夜福利视频在线观看| 天堂影院成人在线观看| 久久久国产成人精品二区| 成人手机av| 久久精品国产亚洲av高清一级| 十八禁网站免费在线| 国产一区二区在线观看日韩 | 黄色 视频免费看| 亚洲欧美精品综合一区二区三区| 99久久99久久久精品蜜桃| 国产又黄又爽又无遮挡在线| 成人国语在线视频| 久久香蕉激情| 国模一区二区三区四区视频 | 久久久久久人人人人人| 国产黄片美女视频| 日韩欧美在线乱码| 国产精品一区二区免费欧美| 性欧美人与动物交配| 后天国语完整版免费观看| 国产成人精品无人区| 久久久精品欧美日韩精品| 男女床上黄色一级片免费看| 黄色女人牲交| 国产精品香港三级国产av潘金莲| 亚洲自拍偷在线| 国内少妇人妻偷人精品xxx网站 | 欧美高清成人免费视频www| 成人一区二区视频在线观看| 成人18禁高潮啪啪吃奶动态图| 在线国产一区二区在线| 村上凉子中文字幕在线| 亚洲aⅴ乱码一区二区在线播放 | 18禁国产床啪视频网站| 免费av毛片视频| 在线观看一区二区三区| 国产成人系列免费观看| 婷婷精品国产亚洲av在线| 伊人久久大香线蕉亚洲五| 日韩欧美 国产精品| 人妻夜夜爽99麻豆av| 国产99白浆流出| 精品国产超薄肉色丝袜足j| 全区人妻精品视频| 黑人巨大精品欧美一区二区mp4| 精品福利观看| 国产精品一区二区精品视频观看| 色老头精品视频在线观看| 超碰成人久久| 一本综合久久免费| 欧美日韩国产亚洲二区| 亚洲人成77777在线视频| 变态另类丝袜制服| 久久久水蜜桃国产精品网| 亚洲精品美女久久av网站| 亚洲精品美女久久av网站| 久久久水蜜桃国产精品网| a级毛片在线看网站| 一个人观看的视频www高清免费观看 | 九九热线精品视视频播放| 久久精品综合一区二区三区| 欧美日韩中文字幕国产精品一区二区三区| 天堂√8在线中文| 国产午夜精品久久久久久| 国产精品日韩av在线免费观看| av有码第一页| 90打野战视频偷拍视频| videosex国产| 国产精品久久久av美女十八| 一区二区三区高清视频在线| 国产精品乱码一区二三区的特点| 又黄又粗又硬又大视频| 亚洲最大成人中文| 亚洲色图av天堂| 又紧又爽又黄一区二区| 久久精品91蜜桃| 老司机靠b影院| 国产三级中文精品| 久久人人精品亚洲av| 欧美av亚洲av综合av国产av| 午夜福利欧美成人| 日本 av在线| 在线免费观看的www视频| 99在线人妻在线中文字幕| 国产精品一区二区三区四区久久| 黄色视频不卡| 丝袜美腿诱惑在线| 中亚洲国语对白在线视频| 国产av麻豆久久久久久久| 久久久久久人人人人人| 免费高清视频大片| 午夜福利视频1000在线观看| 精品久久久久久久久久久久久| 亚洲精品一卡2卡三卡4卡5卡| 一区福利在线观看| 18禁裸乳无遮挡免费网站照片| 真人一进一出gif抽搐免费| 非洲黑人性xxxx精品又粗又长| 精品午夜福利视频在线观看一区| 一本精品99久久精品77| 黄色a级毛片大全视频| 人人妻人人看人人澡| 免费在线观看视频国产中文字幕亚洲| av免费在线观看网站| ponron亚洲| 日韩 欧美 亚洲 中文字幕| 久久天堂一区二区三区四区| 床上黄色一级片| 狠狠狠狠99中文字幕| 男插女下体视频免费在线播放| 国内精品久久久久精免费| 亚洲国产精品999在线| 我要搜黄色片| 欧美成人免费av一区二区三区| www日本在线高清视频| 啦啦啦免费观看视频1| 狠狠狠狠99中文字幕| 欧美极品一区二区三区四区| 亚洲午夜精品一区,二区,三区| 香蕉av资源在线| 中文字幕熟女人妻在线| 国产成人影院久久av| aaaaa片日本免费| 中文在线观看免费www的网站 | 国产精品av视频在线免费观看| 国产一区二区在线av高清观看| 人成视频在线观看免费观看| 国产真实乱freesex| 欧美极品一区二区三区四区| 亚洲 欧美一区二区三区| www日本在线高清视频| 免费在线观看影片大全网站| www日本黄色视频网| 99在线人妻在线中文字幕| cao死你这个sao货| 日本一区二区免费在线视频| 法律面前人人平等表现在哪些方面| 日日摸夜夜添夜夜添小说| av免费在线观看网站| 亚洲精品在线观看二区| 久久精品国产清高在天天线| 亚洲性夜色夜夜综合| 这个男人来自地球电影免费观看| 久久久久性生活片| 黑人欧美特级aaaaaa片| 少妇熟女aⅴ在线视频| 国内少妇人妻偷人精品xxx网站 | 国产69精品久久久久777片 | 亚洲av熟女| 在线观看免费午夜福利视频| 欧洲精品卡2卡3卡4卡5卡区| 特大巨黑吊av在线直播| 蜜桃久久精品国产亚洲av| 看片在线看免费视频| 国产精品98久久久久久宅男小说| 91字幕亚洲| 午夜a级毛片| 露出奶头的视频| 色播亚洲综合网| 国产麻豆成人av免费视频| 日韩欧美在线二视频| 色综合婷婷激情| 欧美三级亚洲精品| 五月伊人婷婷丁香| 九色成人免费人妻av| 欧美黑人巨大hd| 国内精品久久久久久久电影| 天堂影院成人在线观看| 在线观看舔阴道视频| 久久久久国产精品人妻aⅴ院| 国产成人aa在线观看| 成人亚洲精品av一区二区| 日日夜夜操网爽| 国产黄片美女视频| 国产三级在线视频| 久久精品影院6| 母亲3免费完整高清在线观看| 日本一区二区免费在线视频| 欧美黄色淫秽网站| 亚洲精品国产一区二区精华液| 波多野结衣巨乳人妻| 国产视频一区二区在线看| 久久人人精品亚洲av| 岛国视频午夜一区免费看| 69av精品久久久久久| 国内精品久久久久久久电影| 高潮久久久久久久久久久不卡| 婷婷精品国产亚洲av| 97人妻精品一区二区三区麻豆| 90打野战视频偷拍视频| 香蕉国产在线看| 国产片内射在线| 亚洲国产精品合色在线| 熟女电影av网| 欧美在线黄色| 久久久久久大精品| 真人一进一出gif抽搐免费| 日本三级黄在线观看| 国产伦在线观看视频一区| 久热爱精品视频在线9| 亚洲欧美日韩无卡精品| 国产一区二区激情短视频| 一边摸一边抽搐一进一小说| 久久久久国产一级毛片高清牌| 日韩欧美在线乱码| 男人舔女人的私密视频| 免费在线观看完整版高清| 欧美zozozo另类| 老司机午夜十八禁免费视频| 91大片在线观看| 婷婷精品国产亚洲av| 丁香欧美五月| 长腿黑丝高跟| 成人手机av| 亚洲第一电影网av| 国产精品一区二区三区四区免费观看 | 日韩av在线大香蕉| 国产精品国产高清国产av| 免费高清视频大片| 国产单亲对白刺激| 精品不卡国产一区二区三区| 亚洲av美国av| 很黄的视频免费| 在线a可以看的网站| 亚洲狠狠婷婷综合久久图片| 亚洲人成电影免费在线| 成人一区二区视频在线观看| 欧美日韩黄片免| 哪里可以看免费的av片| 亚洲欧美日韩高清专用| 精品国产乱子伦一区二区三区| 国产午夜福利久久久久久| 久久久久久久久久黄片| 91国产中文字幕| xxx96com| 久久婷婷成人综合色麻豆| 美女黄网站色视频| 久久精品成人免费网站| 一卡2卡三卡四卡精品乱码亚洲| 无限看片的www在线观看| 国产亚洲精品第一综合不卡| 淫秽高清视频在线观看| bbb黄色大片| 亚洲熟女毛片儿| 国产精品日韩av在线免费观看| 一卡2卡三卡四卡精品乱码亚洲| 亚洲中文字幕一区二区三区有码在线看 | 少妇熟女aⅴ在线视频| 五月玫瑰六月丁香| 最新在线观看一区二区三区| 中文字幕高清在线视频| 亚洲乱码一区二区免费版| а√天堂www在线а√下载| 色综合欧美亚洲国产小说| 亚洲av五月六月丁香网| 国产蜜桃级精品一区二区三区| 这个男人来自地球电影免费观看| 欧美久久黑人一区二区| 老汉色∧v一级毛片| 琪琪午夜伦伦电影理论片6080| 免费在线观看亚洲国产| 超碰成人久久| 国产精品av视频在线免费观看| cao死你这个sao货| 亚洲avbb在线观看| 国产精品98久久久久久宅男小说| 国产av一区二区精品久久| 久久久久国内视频| 国产aⅴ精品一区二区三区波| 欧美日韩黄片免| 视频区欧美日本亚洲| 亚洲一区高清亚洲精品| 搞女人的毛片| 草草在线视频免费看| 久久九九热精品免费| 日日夜夜操网爽| 国产亚洲精品第一综合不卡| 两个人视频免费观看高清| 国产精品永久免费网站| 亚洲精品在线美女| 亚洲av日韩精品久久久久久密| 久久久久久亚洲精品国产蜜桃av| 亚洲国产精品合色在线| 国产蜜桃级精品一区二区三区| 两性夫妻黄色片| 麻豆一二三区av精品| 丁香欧美五月| 桃红色精品国产亚洲av| 一级毛片高清免费大全| 亚洲成人中文字幕在线播放| 1024视频免费在线观看| 成人一区二区视频在线观看| 亚洲美女黄片视频| 欧美成人一区二区免费高清观看 | 18禁黄网站禁片午夜丰满| 两性午夜刺激爽爽歪歪视频在线观看 | 日韩 欧美 亚洲 中文字幕| 99riav亚洲国产免费| 亚洲av中文字字幕乱码综合| 久久久久亚洲av毛片大全| 人成视频在线观看免费观看| 最新美女视频免费是黄的| 欧美一区二区精品小视频在线| 精品国产乱码久久久久久男人| 欧美中文综合在线视频| 亚洲中文字幕一区二区三区有码在线看 | 午夜精品一区二区三区免费看| 999久久久国产精品视频| 69av精品久久久久久| 免费在线观看日本一区| 一级a爱片免费观看的视频| 在线观看免费日韩欧美大片| 久久精品国产综合久久久| 少妇被粗大的猛进出69影院| 国产麻豆成人av免费视频| 手机成人av网站| 国产精品九九99| 亚洲男人的天堂狠狠| 日韩欧美 国产精品| 久久精品国产亚洲av高清一级| 亚洲欧洲精品一区二区精品久久久| 午夜福利在线在线| 日韩高清综合在线| 亚洲国产日韩欧美精品在线观看 | 免费看十八禁软件| netflix在线观看网站| 88av欧美| 亚洲精品国产一区二区精华液| 欧美一区二区精品小视频在线| 久久久久久久精品吃奶| 99国产精品99久久久久| 免费av毛片视频| 首页视频小说图片口味搜索| 日韩中文字幕欧美一区二区| 我要搜黄色片| 免费在线观看日本一区| 国产精品香港三级国产av潘金莲| 无人区码免费观看不卡| 黑人巨大精品欧美一区二区mp4| 嫩草影院精品99| 亚洲在线自拍视频| 色噜噜av男人的天堂激情| 免费在线观看黄色视频的| 又紧又爽又黄一区二区| 我要搜黄色片| 国产av麻豆久久久久久久| 少妇被粗大的猛进出69影院| 最新在线观看一区二区三区| 久久婷婷成人综合色麻豆| 日本 欧美在线| 亚洲自偷自拍图片 自拍|