    Modification Mechanism of Coconut Husk Activated Carbon Using FeSO4 and Fe(NO3)3

    2020-10-26 08:33:12HUANGBangfu1LIULanpeng1WANGDefu1LILu李露

    HUANGBangfu1,2*,LIULanpeng1,2,WANGDefu1,2,LILu(李露)1,2

    1 Department of Metallurgical Engineering, Kunming University of Science and Technology, Kunming 650093, China2 Clean Metallurgy Key Laboratory of Complex Iron Resources, University of Yunnan Province, Kunming 650093, China

    Abstract: Modification conditions determine the surface topography and the active material phase composition of a catalyst. To study the influence of modification on a carbon-based sorbent, coconut husk activated carbon (AC) which was activated using HNO3 and modified by FeSO4 and Fe(NO3)3 was examined. The pore textures and surface chemical characteristics of the carbon materials were examined by scanning electron microscopy(SEM), Brunner-Emmet-Teller(BET), X-ray diffraction (XRD) and Fourier transform infrared (FTIR) spectroscopy. The surface topography, the pore structure, active materials, and functional groups of AC, AC modificated by HNO3 (HNO3/AC for short), and AC modificated by FeSO4 and Fe(NO3)3 (Fe/AC for short) were systematically studied. Subsequently, the mechanism of modifying the conditions for the carbon materials was determined. Results showed that the surface micro topography of HNO3/AC became unsystematic and disordered. After modification with FeSO4, the ferriferous oxide was mainly present as a near-spherical crystal. Ferriferous oxides from Fe(NO3)3 modification mainly exhibited a plate shape. HNO3 modification could enlarge the pores but decrease the specific surface area of AC. FeSO4 modification resulted in a new net post structure in the pore canal of AC. Fe(NO3)3 modification caused the pore space structure to develop in the interior, and a higher calcination temperature was useful for ablation. The ash content of the AC was substantially reduced upon HNO3 modification. Upon FeSO4 modification, α-FeOOH, α-Fe2O3 and γ-Fe2O3 coexisted under the condition of a lower concentration of FeSO4 and a lower calcination temperature, and a higher FeSO4 concentration and calcination temperature generated more α-Fe2O3. The same Fe(NO3)3 modification and a higher calcination temperature were beneficial to the minor chipping formation of γ-Fe2O3. A higher Fe(NO3)3 loading produced a lower graphitization degree. HNO3 modification formed various new oxygen-containing functional groups and few nitrogen-containing groups. Based on the cover, FeSO4 and Fe(NO3)3 modification could decrease the oxygen-containing and nitrogen-containing functional groups. These results could optimize the modification condition and improve physical and chemical properties of carbon-based sorbents.

    Key words: HNO3; FeSO4; Fe(NO3)3; coconut husk activated carbon; characterization; modification mechanism

    Introduction

    Activated carbon (AC) is a good catalyst carrier, and it presents with a large specific surface area and many pores[1-2]. The surface of AC exhibits many oxygen-containing and nitrogen-containing functional groups. AC demonstrates stable chemical properties, and is acid-resistant, alkali-resistant and renewable. Thus, as an adsorbing material, AC is widely used in gas cleaning, catalysis, medicine and chemical engineering fields[3-5]. Coconut husk AC exhibits favorable adsorptive properties, a high mechanical strength, and stable chemical properties. The adsorption capacity and catalytic performance of coconut husk AC are determined by the pore structure and surface functional groups. Unmodified coconut husk AC exhibits limited adsorptive properties compared with modified coconut husk AC. As a result, coconut husk AC should be modified by materials that demonstrate a high catalytic activity to increase its physicochemical adsorption capacity.

    The previous study[6]has shown that AC modified by nitric acid possesses appropriate acidity-basicity and increases the oxygen-containing functional groups, which destroys the pore structure and increases Br?nsted acid sites and Lewis acid sites. The main metallic modification compounds include FeOx, CuOx, MnOxand CeOx[7-10], and these provide AC with low-temperature catalytic activity. In particular, the active metal oxide, FeOx, is an iron-based catalyst with a broad active temperature window, good selective catalytic reduction (SCR) capability, high N2selectivity, high low-temperature water resistance and high acidic active sites[11-12]. Therefore, AC modified with FeOxexhibits good physicochemical properties. However, the preparation conditions determine the Fe phase composition and physicochemical properties of the catalyst.

    To study the influence of the modification conditions, coconut husk ACs activated with HNO3and modified using FeSO4and Fe(NO3)3were examined, respectively. The pore texture and surface chemical characteristics of the carbon materials were examined via scanning electron microscopy (SEM), Brunner-Emmet-Teller (BET), X-ray diffraction (XRD) and Fourier transform infrared (FTIR) spectroscopy. The physicochemical properties of AC, AC modified through HNO3(HNO3/AC) and AC modified through FeSO4and Fe(NO3)3(Fe/AC) were systematically studied.

    1 Experiments

    1.1 Catalyst preparation

    Coconut husk AC (Chongqing Huaxi Cativated Create Factory, Chongqing, China) was used as the raw carbon material. The coconut husk AC was washed with distilled water and soaked in a water bath for 2 h. Then, the AC sample was dried in an oven at 100 ℃. The AC sample was immersed in 4.0 mol/L HNO3at 80 ℃ for 2 h. Then, HNO3/AC was obtained by drying the sample in an oven at 100 ℃.

    The HNO3/AC sample (10 g) was first immersed in FeSO4liquor (100 mL), and the mixture was treated with supersonic at 60 ℃ for 2 h and stewed for 12 h. Afterwards, FeSO4liquor was added to 2 mol/L ammonia and 10% H2O2,and then the Fe(OH)3precipitate was obtained by stirring at 55 ℃ for 1 h. The Fe(OH)3precipitate was suction filtrated and dried at 55 ℃ for 12 h. The dried sample was calcined in a vacuum tube furnace. The catalyst samples were washed with distilled water three times and dried at 55 ℃ for 12 h. Details of the FeSO4modification conditions are provided in Table 1.

    Table 1 Catalyst preparation conditions

    Based on the water absorbing capacity of HNO3/AC, 10 g HNO3/AC was first immersed in isometric Fe(NO3)3and stewed for 24 h, and then the mixture was dried in an oven at 100 ℃ for 4 h. Afterwards, the dried sample was calcined in a vacuum tube furnace in N2atmosphere for 3 h. Details of the Fe(NO3)3modified conditions are provided in Table 1.

    1.2 Materials characterization

    To study the changes in the surface topographies of AC, HNO3/AC and Fe/AC, the microstructures of the carbon materials were observed by SEM (VEGA 3 SBU/VEGA 3 SBH, Tescan Orsay Holding, China). The pore diameters affected the physical adsorption capability. The BET surface areas of the samples before and after modifications were measured using the N2adsorption isotherm through the nitrogen adsorption desorption tester (QuadraSorb SI,Quantachrome Instruments, America). Volumes of total pores and micropores were obtained using the Barclay-James-Harvest (BJH) method. The characteristic structural parameters, including the pore-size distributionD, the volume of total poresVtotal, the volume of microporesVmicro, the specific surface area of total poresStotaland the specific surface area of microporesSmicro, were obtained by analyzing the adsorption tendency. The Fe phase composition was observed through XRD (TTR III, Beijing Advance Science & Technology Corporation, China). The species and the amounts of surface functional groups affected the surface chemical properties. To study the changes in the surface functional groups of AC, HNO3/AC and Fe/AC, FTIR spectra were recorded using a FTIR spectrometer (Nicolet iS10, Thermo Fisher Scientific, China).

    2 Results and Discussion

    2.1 SEM characterization

    The surface micro topographies of the samples before and after modifications with HNO3are shown in Figs. 1(a) and (b). Figure 1(a) shows that AC develops a pore structure, a distinct boundary, a smooth wall of holes and a faviform surface structure. Figure 1(b) shows that the surface micro topography of HNO3/AC becomes unsystematic and disordered, and the same area presents more ditches and air void structures compared to that of AC. Meanwhile, some gully-like pores are formed on the surface of HNO3/AC.

    (a)

    (b)

    The SEM images for Fe/AC-1, Fe/AC-2 and Fe/AC-3 are shown in Fig. 2.

    (a)

    (b)

    (c)

    (d)

    (e)

    (f)

    For Fe/AC-1 in Figs. 2(a) and (b), the ferriferous oxide shows a serious birdnesting phenomenon upon Fe(OH)3modification at 200 ℃ for calcination. The birdnesting phenomenon is as follows: a birdnesting lump attaches to the hole wall of AC with poor dispersivity; a birdnesting object accumulates on the surface of AC in a random manner and blocks part of the pore canal; the active material of ferriferous oxide coagulates in lumps and exhibits a sharp nonuniformity.

    Figures 2(c) and (d) of Fe/AC-2 show that reticulate and prismatical crystals develop between the pore space of AC. Some of the crystals connect the top and the bottom pore walls, whereas others show a continuous growth. The reticulate and prismatical crystals of ferriferous oxide form a new pore path structure, which makes the inner space of AC be fully utilized. Therefore, Fe/AC-2 exhibits a larger specific surface area compared with AC and HNO3/AC. Meanwhile, on the surface of Fe/AC-2, the serious birdnesting phenomenon which is obvious in Fe/AC-1 disappears, and crystal grains replace the birdnesting phenomenon,present globosity, and are oval in shape. Thus, the good dispersivity of the crystal grains on the surface also increases the specific surface area of Fe/AC-2. For Fe/AC-2, there is no serious plug-hole phenomenon on the surface or in the pore space, and it could supply a larger specific surface area and more active adsorption sites.

    For Fe/AC-3, as shown in Figs. 2(e) and (f), the surface of Fe/AC-3 becomes sunken, smashed and rough when the density of FeSO4increases and when the calcination temperature is 250 ℃. The ferriferous oxide of Fe/AC-3 adheres on the surface and accumulates in the pore space compared with Fe/AC-1 that accumulates on the surface. Moreover, most ferriferous oxide shows graininess, and few ferriferous oxide shows bond lumps and adheres on the surface of the pore path to create blockages.

    The surface morphologies of Fe/AC-4, Fe/AC-5 and Fe/AC-6 modified with Fe(NO3)3isometric impregnation and high-temperature calcination are shown in Fig. 3.

    (a)

    (b)

    (d)

    For Fe/AC-4 in Figs. 3(a) and (b), the surface exhibits a certain thickness and lumps of ferriferous oxide, and many cracks in the ferriferous oxide exist. This may be due to the formation of NO2and O2when Fe(NO3)3begins to decompose upon high-temperature calcination. Moreover, some of the powdery accumulation and graininess of the irregular crystals of ferriferous oxide accrete on the hole surfaces of the AC, and less lumps of Fe2O3are present in the holes.

    In comparison with Figs. 3(a) and (b), the pore structure of Fe/AC-5 is highly visible as the calcination temperature increases. This may be because the lumps of ferriferous oxide split into fine-grained chippings that spread out on the surface and the pore structure of AC. Furthermore, part of the fine-grained chippings inlays the pore holes. Consequently, the specific surface area and the micropore area are enlarged, which are favorable for increasing the adsorptive property.

    The surface of Fe/AC-6 becomes crude and messy as the loading amount increases at a constant calcination temperature. Compared with Fe/AC-4, the ferriferous oxide of Fe/AC-6 is in big lumps attached to the surface of AC. Some minor micropores on the surface of the big lumps exist, and the shape of catalysts is irregular. Many ferriferous oxide crystals go into the pore structure of AC and create more pore paths.

    Thus, ferriferous oxide from Fe/AC-1, Fe/AC-2 and Fe/AC-3 is mainly present as a near-spherical crystal, which forms a new net post structure in the pore canal. At the same loading concentration of FeSO4, the higher calcination temperature causes more scattered ferriferous oxide, which supplies a larger specific surface area and more adsorption active sites. For the same calcination temperature for FeSO4, a higher loading amount causes ferriferous oxide to become sunken, smashed and rough. Ferriferous oxide in Fe/AC-4, Fe/AC-5 and Fe/AC-6 is mainly present as a plate shape and adheres on the surface of Fe/AC. When the same loading amount of Fe(NO3)3is used, a higher calcination temperature causes minor chippings of ferriferous oxide, which spreads out on the surface and pore space. When the same calcination temperature is used for Fe(NO3)3, a higher loading amount results in more bulk mass ferriferous oxide, which forms more pore canals.

    2.2 BET characterization

    The BET characterization results for AC, HNO3/AC, and Fe/AC are shown in Table 2.

    Table 2 Specific surface areas and pore structure parameters

    For AC, the diameters of the micropores are almost 2 nm, and the developed micropore structure exhibits an immense specific surface area[13]. Upon calculating, the micropore volume accounts for 69.97% of the total pore volume, and the micropore specific surface area accounts for 83.37% of the total specific surface area. Therefore, mesopores and macropores are rarely present. For HNO3/AC, the average pore diameter and the total pore volume increase slightly after HNO3modification. This is because many closed pores are opened owing to the reaction between HNO3and carbon, which causes some of the micropores to disappear and the carbon skeleton to topple. Therefore, the micropore structure is destroyed, the micropore specific surface area decreases to 190.595 m2/g, and the total specific surface area decreases to 132.604 m2/g. Thus, HNO3modification enlarges the pores but decreases the specific surface area of AC as shown in Fig. 1(b).

    The nitrogen isothermal adsorption-desorption curves and pore size distributions of Fe/AC-1, Fe/AC-2 and Fe/AC-3 are shown in Fig. 4. The adsorbed volumes of N2for Fe/AC-1, Fe/AC-2 and Fe/AC-3 rapidly increase during the initial stage in the low relative pressure, which means that many micropores are present and can be defined as type I according to International Union for Pure and Applied Chemistry (IUPAC) classification[13]. As shown in Figs. 4(a) and (b) and Table 2, the micropore contents are in the following order: Fe/AC-2 > Fe/AC-1 > Fe/AC-3. The adsorbed volume of N2for Fe/AC-1, Fe/AC-2 and Fe/AC-3 also rapidly increases at the high pressure. The reason for this may be that in the narrow free space, capillary condensation occurs under the medium pressure and the high pressure; thus, micropores and mesopores are present. This tendency can be defined as type IV. Condensation and evaporation of capillaries do not occur at the same pressure, which leads to a circular hysteresis ring. The mesopore amount of Fe/AC rapidly increases as the calcination temperature increases. Thus, the high temperature can change the micropores to mesopores; however, a larger increase in micropores is observed. Therefore, the average pore diameters of Fe/AC-1, Fe/AC-2 and Fe/AC-3 decrease to various degrees compared with those of AC and HNO3/AC.

    One possible reason is the large amount of gas prior to the opening up of the inner pore space when the Fe(OH)3calcines and generates gas. Thus, the ferriferous oxide crystals attach to the macropore wall and continuously accumulate. Then, more micropores are formed in the pore canal, which makes the best use of the inner pore space. On the surface, the ferriferous oxide crystals form round-like crystals and enlarge the specific surface area of AC, especially for Fe/AC-2. Because there are more micropores in Fe/AC-2 than in Fe/AC-1 and Fe/AC-3, the pore volume and the specific surface area of Fe/AC-2 exhibit the highest increase; therefore, it can be concluded that the Fe/AC-2 has the strongest adsorption capacity.

    (a)

    (b)

    The nitrogen isothermal adsorption-desorption curves and pore size distributions of Fe/AC-4, Fe/AC-5 and Fe/AC-6 are shown in Fig. 5.

    (a)

    (b)

    As shown in Fig. 5(a), the adsorbed volumes of N2for Fe/AC-4, Fe/AC-5 and Fe/AC-6 also rapidly increase at the high pressure during the initial stage; thus, many micropores are present. As shown in Table 2, from high value to low value, the specific surface areas are Fe/AC-5 > Fe/AC-6 > Fe/AC-4. In addition, some mesopores and narrow spaces are formed by numerous flaky particles. From Table 1, the mesopore number in Fe/AC-4 and Fe/AC-5 rapidly increases as the calcination temperature increases. Thus, the high temperature can change micropores to mesopores, but a larger increase exists in micropores than in mesopores. Therefore, the average pore diameters of Fe/AC-4, Fe/AC-5 and Fe/AC-6 decrease compared to those of AC and HNO3/AC.

    The main reason for the pore diameter change is that the shrinkage of the AC skeleton makes the pore diameter and the channel decrease upon high-temperature calcination and nitrogen protection. The Fe ions could enter the pore space interior of AC via an immersion process. When Fe2O3forms during high-temperature calcination, the crystal positions become a point of heat accumulation and cause the reaction of Fe(NO3)3with the volatile component. Therefore, the pore space structure of AC can develop in the interior, and part of AC is ablated by Fe(NO3)3decomposition. Based on a loading amount of Fe2O3of 5% and a calcination temperature of 500 ℃, Fe/AC-5 is abundantly ablated with the minimum pore diameter, the pore volume and the specific surface area are the maximum, while the adsorption capacity is also the maximum. When the calcination temperature is 400 ℃, the parameters for Fe/AC-4 and Fe/AC-6 are the same. The micropore volume of Fe/AC-6 is less than that of Fe/AC-4, and the micropore specific surface area of Fe/AC-6 is larger than that of Fe/AC-4. This could be attributed to ferriferous oxide supplying more micropores and the specific surface area as the loading amount increases.

    2.3 XRD characterization

    The graphite crystal is the main part of AC. The phase composition of ferriferous oxide loading into AC mainly includes paramagnetismα-Fe2O3and ferromagnetismγ-Fe2O3. To analyze the change in the graphite crystal and the Fe phase composition, the XRD spectra of AC, HNO3/AC and Fe/AC are measured, as shown in Fig. 6.

    As shown in Fig. 6(a), a graphite peak is found in the XRD spectra of AC and HNO3/AC, and there are two characteristic peaks of broad dispersion at 23.813° and 43.467° (100 crystal face). Thus, AC is composed of amorphous carbon. The diffraction peak due to the decompacting and tiering graphene layer is at a 2θof 23.813°. The diffraction peak from the graphite crystal is at a 2θof 43.467°. The diffraction peak from the graphite crystal face of 002 is at a 2θof 26.468°[14]. Thus, the diffraction peaks of the graphene layer and the graphite crystal become keen-edged peaks when AC is modified via nitric acid oxidation. This could be attributed to that the ash content of AC substantially reduced when it is modified with nitric acid, which makes the diffraction peak keen-edged.

    As shown in Fig. 6(b), the diffraction peaks for Fe/AC-1 are at 35.632° and 63.070°, which belong to 311 and 440 crystal faces ofγ-Fe2O3, respectively, according to Joint Committee on Powder Diffraction Standards(JCPDS) card No. 39-1346[15]. The diffraction peaks forα-FeOOH are at 33.116° and 41.223°, which belong to 130 and 140 crystal faces ofα-FeOOH, respectively, according to JCPDS card No. 29-0713. In addition, the diffraction peak forα-Fe2O3is at 33.116°. Thus, the strength of theα-FeOOH peak is likely weak owing to the low content and the unordered structure[12]. Fe(OH)3could not totally transform intoγ-Fe2O3, and at a calcination temperature of 200 ℃,α-FeOOH coexists withα-Fe2O3andγ-Fe2O3.

    (a)

    (b)

    (c)

    The diffraction peaks for Fe/AC-2 are at 30.214°, 35.679°, 43.317°, 53.720°, 57.276° and 62.872°, which belong to 220, 311, 400, 422, 511 and 440 crystal faces ofγ-Fe2O3, respectively. Although the diffraction peaks are comparatively large, the peak shapes are sharp and symmetrical. Theγ-Fe2O3crystal grain is loaded well; however, the diffraction peaks forα-Fe2O3are still at 33.243° and 40.815°[16].

    For an increased loading amount and the same calcination temperature compared with Fe/AC-2, the diffraction peak forγ-Fe2O3for loading in Fe/AC-3 is at 35.547°, and the diffraction peaks forα-Fe2O3are at 33.243°, 40.881°, 49.638°, 53.856° and 63.860°, which belong to 104, 113, 024, 116, and 300 crystal faces, respectively, according to theα-Fe2O3standard JCPDS card No. 33-0664. The proportion ofα-Fe2O3increases as the loading amount increases. Thus,α-FeOOH orγ-Fe2O3is transformed intoα-Fe2O3[17].

    He gathered slowly, moving backwards4 and forwards through the bushes, but always keeping up with her. After a while, he came back to the path. She answered his questions - the children, her job, her parents - but always skirted round the main issue.

    The XRD spectra of Fe/AC-4 are shown in Fig. 6(c), and the diffraction peaks forα-Fe2O3are at 24.123°, 35.569°, 40.791°, 49.378°, 53.988°, 57.409°, 62.381° and 63.929°. The diffraction peaks forγ-Fe2O3are at 30.109°, 33.088° and 43.216°. There is considerableα-Fe2O3and lessγ-Fe2O3loaded in AC when the loading amount of ferriferous oxide is 5% and the calcination temperature is 400 ℃. The ferriferous oxide is mainly present as a plate shape and adheres on the surface of Fe/AC-4.

    As shown in the XRD spectra of Fe/AC-5, the diffraction peaks forγ-Fe2O3are found at 30.378°, 35.735°, 43.412°, 53.879°, 57.732° and 62.991°. The diffraction peak forα-Fe2O3is at 33.236°. The diffraction peak is keen-edged with symmetry at 35.735°. Thus, the active material is mainlyγ-Fe2O3crystals with good crystallization behaviors that are well distributed when the loading amount of ferriferous oxide is 5% and the calcination temperature is 500 ℃. Theγ-Fe2O3crystals exhibit good crystallinity and dispersivity, and result in minor chippings of ferriferous oxide.

    As shown in the XRD spectra of Fe/AC-6, the diffraction peaks forα-Fe2O3are at 24.182°, 33.170°, 35.645°, 40.861°, 43.334°, 49.460°, 54.055°, 57.553°, 62.409° and 63.979°. The diffraction peak forγ-Fe2O3is at 30.255°. The graphite peak for Fe/AC-6 is broader and lower in amplitude compared with that of Fe/AC-4. Muchα-Fe2O3attaches to the surface of AC, which reduces the graphitization degree of AC. The ferriferous oxide of Fe/AC-6 appears in a large area bulk on the surface.

    Thus, for FeSO4modification, to obtain moreγ-Fe2O3, the FeSO4concentration should be 0.5 mol/L, and the calcination temperature needs to be at 250 ℃. Additionally, Fe(NO3)3is favorable forα-Fe2O3formation under the condition of 400 ℃ calcination, andγ-Fe2O3is formed via 500 ℃ calcination. Therefore, the crystal occurrence of Fe(NO3)3after calcination is determined by the calcination temperature. The loading amount of ferriferous oxide determines the graphitization degree, and a higher loading amount results in a lower graphitization degree.

    2.4 FTIR characterization

    The surface chemical properties of AC are determined by the types and the amount of surface functional groups. The surface functional groups of AC mainly include carboxyl groups, phenolic hydroxyl groups, ester groups, ketone groups, and ethyl ether[18-19]. To determine the functional groups, FTIR was used to analyze the changes in the functional groups on the surface of the carbon materials before and after modifications.

    (a)

    (b)

    (c)

    3 Conclusions

    (1) The surface micro topographies of HNO3/AC became unsystematic and disordered. Upon FeSO4modification, the ferriferous oxide was mainly present as a near-spherical crystal. The ferriferous oxide of Fe/AC modified with Fe(NO3)3was mainly present as a plate shape.

    (2) Modification with nitric acid enlarged the pores but decreased the specific surface area of AC. FeSO4modification formed a new net post structure in the pore canals of AC. Fe(NO3)3modification caused pore space structures to develop in the interior, and a higher calcination temperature was favorable for ablation.

    (3) The ash content of AC substantially decreased upon modification with HNO3. For FeSO4modification,α-FeOOH,α-Fe2O3andγ-Fe2O3coexisted under the conditions of a lower concentration and a lower calcination temperature, and a higher FeSO4concentration and calcination temperature generated moreα-Fe2O3. Fe/AC-2 resulted in moreγ-Fe2O3active material. The calcination temperature during Fe(NO3)3modification determined the Fe graphitization degree, and a higher loading amount resulted in a lower graphitization degree.

    国产免费视频播放在线视频| 久热久热在线精品观看| 狠狠精品人妻久久久久久综合| 高清毛片免费看| 妹子高潮喷水视频| 一个人免费看片子| 亚洲,欧美,日韩| 大陆偷拍与自拍| 成人毛片a级毛片在线播放| 制服丝袜香蕉在线| 国内揄拍国产精品人妻在线| 国国产精品蜜臀av免费| 91久久精品国产一区二区成人| 99久久精品国产国产毛片| 日韩 亚洲 欧美在线| 久久97久久精品| 秋霞在线观看毛片| 国产日韩欧美亚洲二区| 久久精品国产鲁丝片午夜精品| 亚洲人成网站在线播| 国产免费一区二区三区四区乱码| 青春草亚洲视频在线观看| 亚洲av男天堂| 26uuu在线亚洲综合色| 日日啪夜夜撸| 91久久精品电影网| 日韩成人伦理影院| 亚洲精品中文字幕在线视频 | 欧美成人精品欧美一级黄| 男人和女人高潮做爰伦理| 毛片一级片免费看久久久久| 91久久精品国产一区二区三区| 一级毛片 在线播放| 日本色播在线视频| 亚洲av日韩在线播放| 久久女婷五月综合色啪小说| 亚洲欧美日韩东京热| 人妻夜夜爽99麻豆av| 一区在线观看完整版| 婷婷色麻豆天堂久久| 亚洲欧美成人精品一区二区| 蜜桃亚洲精品一区二区三区| 91精品伊人久久大香线蕉| 在线观看国产h片| 亚洲av福利一区| 最黄视频免费看| 久久99精品国语久久久| av网站免费在线观看视频| 精品熟女少妇av免费看| 成人免费观看视频高清| 久久久久久久久久成人| 成人午夜精彩视频在线观看| 久久婷婷青草| 精品亚洲成a人片在线观看 | 日本-黄色视频高清免费观看| 午夜日本视频在线| 一级毛片aaaaaa免费看小| 高清视频免费观看一区二区| 人人妻人人澡人人爽人人夜夜| 日韩欧美 国产精品| 99热国产这里只有精品6| 黑人猛操日本美女一级片| 午夜老司机福利剧场| 中文字幕亚洲精品专区| 日韩欧美一区视频在线观看 | 国产一区二区三区综合在线观看 | 免费观看无遮挡的男女| 国产黄色视频一区二区在线观看| 中文字幕免费在线视频6| 不卡视频在线观看欧美| 午夜日本视频在线| 18禁裸乳无遮挡动漫免费视频| 深爱激情五月婷婷| 男人爽女人下面视频在线观看| 极品教师在线视频| 亚洲欧美成人精品一区二区| 日韩,欧美,国产一区二区三区| 街头女战士在线观看网站| 97超视频在线观看视频| 免费观看无遮挡的男女| 亚洲精品国产av蜜桃| 在线观看免费视频网站a站| 欧美人与善性xxx| 成年美女黄网站色视频大全免费 | 久久鲁丝午夜福利片| 三级国产精品欧美在线观看| 99久久中文字幕三级久久日本| 久久青草综合色| 毛片女人毛片| 国产久久久一区二区三区| 在线亚洲精品国产二区图片欧美 | 中文字幕精品免费在线观看视频 | 国产一区二区三区综合在线观看 | 欧美少妇被猛烈插入视频| 啦啦啦中文免费视频观看日本| 一区二区三区乱码不卡18| av在线app专区| 久久亚洲国产成人精品v| 免费观看在线日韩| www.色视频.com| 国产男女内射视频| 日本一二三区视频观看| 99久久人妻综合| 国产精品久久久久久久电影| 少妇人妻久久综合中文| 久久青草综合色| 欧美 日韩 精品 国产| 午夜免费观看性视频| 成人亚洲欧美一区二区av| 交换朋友夫妻互换小说| 日韩中文字幕视频在线看片 | 久久女婷五月综合色啪小说| 欧美bdsm另类| 天美传媒精品一区二区| 能在线免费看毛片的网站| 51国产日韩欧美| 尤物成人国产欧美一区二区三区| 精品酒店卫生间| 成人毛片a级毛片在线播放| 一区二区av电影网| 爱豆传媒免费全集在线观看| 99久久中文字幕三级久久日本| 十分钟在线观看高清视频www | 亚洲欧美日韩卡通动漫| 校园人妻丝袜中文字幕| 欧美一区二区亚洲| av一本久久久久| 成人特级av手机在线观看| 日韩制服骚丝袜av| 久久99热这里只有精品18| 五月伊人婷婷丁香| 国产真实伦视频高清在线观看| 国产精品福利在线免费观看| 亚洲精品久久久久久婷婷小说| 午夜福利高清视频| 这个男人来自地球电影免费观看 | 亚洲av男天堂| 午夜福利影视在线免费观看| 涩涩av久久男人的天堂| 中文资源天堂在线| freevideosex欧美| 国产高清国产精品国产三级 | 大陆偷拍与自拍| 久久影院123| 国产69精品久久久久777片| 黄色欧美视频在线观看| 美女主播在线视频| 国产免费视频播放在线视频| 久久精品国产亚洲av天美| 尾随美女入室| 自拍偷自拍亚洲精品老妇| 国产精品国产三级国产av玫瑰| 老司机影院成人| 国产高清三级在线| 男的添女的下面高潮视频| 日日撸夜夜添| 亚洲精品成人av观看孕妇| 免费人成在线观看视频色| 欧美日韩一区二区视频在线观看视频在线| 国产欧美另类精品又又久久亚洲欧美| 夜夜骑夜夜射夜夜干| 99久久精品一区二区三区| 永久网站在线| 大片电影免费在线观看免费| 久久国内精品自在自线图片| 国产成人一区二区在线| av国产免费在线观看| 亚洲国产精品一区三区| 秋霞在线观看毛片| 网址你懂的国产日韩在线| 自拍偷自拍亚洲精品老妇| 精品一区在线观看国产| 天堂俺去俺来也www色官网| 免费黄频网站在线观看国产| 成人亚洲精品一区在线观看 | 日韩中文字幕视频在线看片 | 永久网站在线| 精品一区二区免费观看| 亚洲va在线va天堂va国产| 成人美女网站在线观看视频| 欧美日韩一区二区视频在线观看视频在线| 亚洲av.av天堂| 人人妻人人添人人爽欧美一区卜 | 蜜桃在线观看..| 日韩人妻高清精品专区| 亚洲内射少妇av| 97精品久久久久久久久久精品| 久久精品熟女亚洲av麻豆精品| 成年美女黄网站色视频大全免费 | 欧美日本视频| av国产免费在线观看| 久久99热这里只频精品6学生| 成年免费大片在线观看| 亚洲性久久影院| 精品国产乱码久久久久久小说| 亚洲欧美日韩卡通动漫| 啦啦啦啦在线视频资源| 久久久久国产网址| 97超视频在线观看视频| 国产人妻一区二区三区在| 日本欧美视频一区| 国产免费福利视频在线观看| 国产精品一区二区在线不卡| 欧美成人精品欧美一级黄| 久久鲁丝午夜福利片| 亚洲精品,欧美精品| 97热精品久久久久久| 中文字幕人妻熟人妻熟丝袜美| 亚洲成人av在线免费| av免费观看日本| 能在线免费看毛片的网站| 丝袜喷水一区| 日韩av不卡免费在线播放| 爱豆传媒免费全集在线观看| 国产精品伦人一区二区| 熟女电影av网| 一级片'在线观看视频| 成人二区视频| www.av在线官网国产| 少妇丰满av| 亚洲精品久久午夜乱码| 一级毛片aaaaaa免费看小| 亚洲激情五月婷婷啪啪| 免费观看性生交大片5| 国产精品国产三级国产专区5o| 久久毛片免费看一区二区三区| 国产黄色免费在线视频| 久久精品久久精品一区二区三区| 热re99久久精品国产66热6| 国产精品久久久久久久电影| 高清av免费在线| 免费黄色在线免费观看| 99热这里只有是精品50| 国产午夜精品久久久久久一区二区三区| 免费观看无遮挡的男女| 精品人妻一区二区三区麻豆| 亚洲av日韩在线播放| 九色成人免费人妻av| 成人影院久久| 国产在线一区二区三区精| 丝袜喷水一区| 亚洲精品久久久久久婷婷小说| 日韩av在线免费看完整版不卡| 免费观看a级毛片全部| 欧美少妇被猛烈插入视频| a级毛色黄片| 欧美+日韩+精品| 爱豆传媒免费全集在线观看| 免费在线观看成人毛片| 亚洲第一区二区三区不卡| 伦理电影免费视频| 中文字幕免费在线视频6| 黑丝袜美女国产一区| 七月丁香在线播放| 免费黄色在线免费观看| 国产精品麻豆人妻色哟哟久久| av在线观看视频网站免费| 久久精品久久精品一区二区三区| 丝袜喷水一区| 日本av免费视频播放| 在线观看美女被高潮喷水网站| 国产欧美日韩一区二区三区在线 | 22中文网久久字幕| 在线观看国产h片| 国产精品蜜桃在线观看| 精品少妇黑人巨大在线播放| 精华霜和精华液先用哪个| 国产精品久久久久久av不卡| 国产在视频线精品| 国产成人a区在线观看| 亚洲精品久久久久久婷婷小说| 午夜免费鲁丝| 国产欧美日韩一区二区三区在线 | 中文字幕亚洲精品专区| 久久久久久久久久人人人人人人| 九九久久精品国产亚洲av麻豆| 嫩草影院入口| 熟女人妻精品中文字幕| 麻豆成人av视频| 婷婷色麻豆天堂久久| 日日摸夜夜添夜夜爱| 99热这里只有精品一区| 午夜日本视频在线| 亚洲高清免费不卡视频| 嘟嘟电影网在线观看| 老师上课跳d突然被开到最大视频| 嫩草影院入口| 建设人人有责人人尽责人人享有的 | 99热6这里只有精品| 亚洲av中文字字幕乱码综合| 精品国产三级普通话版| 一级毛片久久久久久久久女| 欧美一级a爱片免费观看看| 一个人看的www免费观看视频| 五月玫瑰六月丁香| 下体分泌物呈黄色| 91狼人影院| 九九久久精品国产亚洲av麻豆| 日本一二三区视频观看| 国产伦理片在线播放av一区| 精品一区二区免费观看| 一级黄片播放器| 看十八女毛片水多多多| 精品国产乱码久久久久久小说| 高清欧美精品videossex| 少妇的逼水好多| 一区二区三区精品91| 亚洲婷婷狠狠爱综合网| 欧美日本视频| av免费在线看不卡| 丝袜脚勾引网站| 99国产精品免费福利视频| 少妇被粗大猛烈的视频| 丰满乱子伦码专区| 午夜激情福利司机影院| 亚洲第一区二区三区不卡| 一级毛片电影观看| 亚洲精品乱码久久久v下载方式| 三级国产精品欧美在线观看| 久久久久精品久久久久真实原创| 丰满迷人的少妇在线观看| 久久久久久久国产电影| 久久久亚洲精品成人影院| 久久精品久久精品一区二区三区| 久久久久久久亚洲中文字幕| 亚洲精品,欧美精品| 男男h啪啪无遮挡| 在线播放无遮挡| 亚洲国产av新网站| 国产成人免费观看mmmm| 麻豆乱淫一区二区| 网址你懂的国产日韩在线| 777米奇影视久久| 亚洲精品中文字幕在线视频 | 国产av国产精品国产| 成人一区二区视频在线观看| 亚洲自偷自拍三级| 日日啪夜夜爽| 午夜福利在线在线| 国产人妻一区二区三区在| 丝瓜视频免费看黄片| 国产真实伦视频高清在线观看| 一级毛片久久久久久久久女| 精品午夜福利在线看| 最近的中文字幕免费完整| av视频免费观看在线观看| 国产成人91sexporn| 国产美女午夜福利| 亚洲久久久国产精品| 中文天堂在线官网| 国产国拍精品亚洲av在线观看| 中文字幕亚洲精品专区| 乱码一卡2卡4卡精品| 亚洲精品视频女| 成人漫画全彩无遮挡| 新久久久久国产一级毛片| 国产亚洲5aaaaa淫片| 国产成人a∨麻豆精品| 亚洲av免费高清在线观看| 日本黄色日本黄色录像| 亚洲综合色惰| 啦啦啦视频在线资源免费观看| 91精品伊人久久大香线蕉| 国产在线一区二区三区精| 国产精品成人在线| 国产 精品1| 国产伦在线观看视频一区| 色婷婷av一区二区三区视频| 韩国高清视频一区二区三区| 亚洲国产高清在线一区二区三| 精品午夜福利在线看| 久久精品国产亚洲av天美| 欧美xxⅹ黑人| 国产成人免费无遮挡视频| 亚洲国产精品国产精品| 国产伦理片在线播放av一区| 22中文网久久字幕| 丰满少妇做爰视频| 午夜免费男女啪啪视频观看| 日韩一本色道免费dvd| 国精品久久久久久国模美| 国产在线一区二区三区精| 日韩av在线免费看完整版不卡| 成人无遮挡网站| 在线播放无遮挡| 亚洲av男天堂| 久久99热6这里只有精品| 永久网站在线| 日韩中文字幕视频在线看片 | 熟女电影av网| 国产精品人妻久久久影院| 如何舔出高潮| 男女边摸边吃奶| 免费观看性生交大片5| 免费看不卡的av| 五月伊人婷婷丁香| 亚洲成人一二三区av| av网站免费在线观看视频| 亚洲色图综合在线观看| 国产精品99久久久久久久久| 99久久中文字幕三级久久日本| 最近最新中文字幕大全电影3| 又大又黄又爽视频免费| 免费黄网站久久成人精品| 国产女主播在线喷水免费视频网站| 噜噜噜噜噜久久久久久91| 欧美日本视频| 搡老乐熟女国产| 少妇精品久久久久久久| 黑人高潮一二区| 直男gayav资源| 国产一区亚洲一区在线观看| 国产成人aa在线观看| 亚洲av欧美aⅴ国产| 最后的刺客免费高清国语| 亚洲国产高清在线一区二区三| 一级毛片电影观看| 男人添女人高潮全过程视频| 亚洲欧洲日产国产| 久久久久久久国产电影| 国产精品无大码| 在线 av 中文字幕| 精品一品国产午夜福利视频| 欧美精品人与动牲交sv欧美| 麻豆乱淫一区二区| 夫妻性生交免费视频一级片| 激情 狠狠 欧美| 小蜜桃在线观看免费完整版高清| 日日撸夜夜添| 午夜老司机福利剧场| 伊人久久国产一区二区| 26uuu在线亚洲综合色| 久久久久视频综合| 99热6这里只有精品| 黄色一级大片看看| 人人妻人人添人人爽欧美一区卜 | 99久久中文字幕三级久久日本| 精品一区二区三区视频在线| 亚洲,欧美,日韩| 91久久精品电影网| 我要看黄色一级片免费的| 亚洲三级黄色毛片| 免费高清在线观看视频在线观看| 干丝袜人妻中文字幕| 亚洲真实伦在线观看| 18禁裸乳无遮挡动漫免费视频| 久久久久久久亚洲中文字幕| 一本色道久久久久久精品综合| 日韩 亚洲 欧美在线| 欧美变态另类bdsm刘玥| 国产精品福利在线免费观看| 免费在线观看成人毛片| 亚洲色图av天堂| 日本av手机在线免费观看| 另类亚洲欧美激情| 国产成人精品久久久久久| 夫妻午夜视频| 人妻 亚洲 视频| 日韩中字成人| 天堂8中文在线网| 午夜福利影视在线免费观看| 久久久久久久久久人人人人人人| 成人特级av手机在线观看| 日本欧美视频一区| 精品国产三级普通话版| 少妇裸体淫交视频免费看高清| 欧美精品亚洲一区二区| 国产在线免费精品| 久久综合国产亚洲精品| 六月丁香七月| 久热久热在线精品观看| av专区在线播放| 精品人妻视频免费看| 老司机影院成人| 免费看光身美女| 青青草视频在线视频观看| 日韩亚洲欧美综合| 亚洲在久久综合| 欧美性感艳星| 熟女av电影| 一级a做视频免费观看| 久久久a久久爽久久v久久| 国产 一区精品| 欧美丝袜亚洲另类| 欧美三级亚洲精品| 久久影院123| 国产伦理片在线播放av一区| 男女边吃奶边做爰视频| 一级a做视频免费观看| 久久国产精品男人的天堂亚洲 | 国产女主播在线喷水免费视频网站| 深夜a级毛片| 在线观看免费高清a一片| 亚洲av在线观看美女高潮| 精品视频人人做人人爽| 亚洲欧美日韩无卡精品| 久久久色成人| 91午夜精品亚洲一区二区三区| 干丝袜人妻中文字幕| 国产精品无大码| 又爽又黄a免费视频| 亚洲av成人精品一二三区| 精品人妻熟女av久视频| 我的老师免费观看完整版| av不卡在线播放| 国产精品久久久久久av不卡| 超碰97精品在线观看| 亚洲美女视频黄频| 成年人午夜在线观看视频| 你懂的网址亚洲精品在线观看| 水蜜桃什么品种好| 久久久久久久久久成人| 视频中文字幕在线观看| 国产av一区二区精品久久 | 纵有疾风起免费观看全集完整版| 大香蕉97超碰在线| 国产有黄有色有爽视频| 啦啦啦中文免费视频观看日本| 99国产精品免费福利视频| h日本视频在线播放| 男女下面进入的视频免费午夜| 亚洲国产色片| 久久女婷五月综合色啪小说| 一二三四中文在线观看免费高清| 免费观看无遮挡的男女| 成人免费观看视频高清| 好男人视频免费观看在线| 99视频精品全部免费 在线| 国模一区二区三区四区视频| 国产亚洲av片在线观看秒播厂| 菩萨蛮人人尽说江南好唐韦庄| 久久精品久久久久久久性| 国产亚洲5aaaaa淫片| 久久精品国产鲁丝片午夜精品| 精品一区二区三卡| 99久久精品热视频| 国产欧美日韩一区二区三区在线 | 嫩草影院新地址| 天堂俺去俺来也www色官网| 国产高清三级在线| 寂寞人妻少妇视频99o| 五月天丁香电影| 精品人妻视频免费看| 女性被躁到高潮视频| 久久精品熟女亚洲av麻豆精品| 26uuu在线亚洲综合色| 国产美女午夜福利| 久久精品熟女亚洲av麻豆精品| 一区在线观看完整版| 亚洲人成网站在线播| www.色视频.com| 我要看日韩黄色一级片| 另类亚洲欧美激情| 搡老乐熟女国产| 日韩成人伦理影院| 国产一区二区三区av在线| 熟妇人妻不卡中文字幕| 亚洲欧美成人综合另类久久久| 亚洲精品中文字幕在线视频 | 色网站视频免费| 国精品久久久久久国模美| 国产毛片在线视频| 中国三级夫妇交换| 国产精品麻豆人妻色哟哟久久| 99re6热这里在线精品视频| 三级国产精品欧美在线观看| 97在线视频观看| 亚洲精品国产av蜜桃| 在线观看一区二区三区| 秋霞伦理黄片| 狂野欧美激情性xxxx在线观看| 久久毛片免费看一区二区三区| 一级毛片久久久久久久久女| 国产在线视频一区二区| 卡戴珊不雅视频在线播放| 成人免费观看视频高清| 能在线免费看毛片的网站| 国产精品久久久久久久电影| 国产亚洲欧美精品永久| 九草在线视频观看| 国产男女内射视频| 另类亚洲欧美激情| 国产高清有码在线观看视频| 夫妻性生交免费视频一级片| 亚洲自偷自拍三级| 欧美 日韩 精品 国产| 又大又黄又爽视频免费| 亚洲欧美中文字幕日韩二区| 男的添女的下面高潮视频| 99热6这里只有精品| 精品少妇黑人巨大在线播放| 女人十人毛片免费观看3o分钟| 夫妻性生交免费视频一级片| 18禁裸乳无遮挡免费网站照片| 永久免费av网站大全| 在线观看三级黄色| 黄色欧美视频在线观看| 欧美日韩在线观看h| 欧美3d第一页| 亚洲av国产av综合av卡| 久久国产亚洲av麻豆专区| 国产v大片淫在线免费观看| 少妇的逼水好多| 草草在线视频免费看| 国产精品国产三级国产专区5o| 日本午夜av视频| 一本一本综合久久| 久久99蜜桃精品久久| 99热6这里只有精品| 国产在线视频一区二区| 久久99热这里只频精品6学生| 水蜜桃什么品种好| 一区二区三区精品91| 婷婷色av中文字幕| 午夜日本视频在线|