    Temperature influences of the recoil characteristics for aluminum honeycomb buffer in the tether-net launcher

    2023-12-07 13:21:50WenhuiShiShuiYueChunWuZhouLiuZhiLiuBeieiZhoZhonghuDuGungGo
    Defence Technology 2023年11期

    Wen-hui Shi ,Shui Yue ,* ,Chun-o Wu ,Zhou Liu ,Zhi Liu ,Bei-ei Zho ,Zhong-hu Du ,Gung-f Go

    a School of Mechanical Engineering, Nanjing University of Science and Technology, Nanjing, 210094, China

    b Aerospace System Engineering Shanghai, Shanghai, 201109, China

    c Xi'an North Qinghua Electromechancal Co., LTD, Xi'an, 710038, China

    Keywords: Tether-net launcher Temperature Aluminum honeycomb buffer Interior ballistic responses Launch recoil characteristics

    ABSTRACT Fluctuations in outer space's temperature would affect the spacecraft's regular operation.This paper aims to study the temperature influences of the aluminum honeycomb buffer in the tether-net launcher.Firstly,a buffer structure was designed to attenuate the pyroshock generated by the pyrotechnic device.Secondly,the mechanical properties of aluminum honeycomb at different temperatures were obtained through quasi-static compression experiments.Then,the internal ballistic responses of the launcher were gained by the closed bomb tests and the equivalent classical interior ballistic model.Finally,the recoil performance of the launcher with aluminum honeycomb buffer at different temperatures was studied.It is revealed that the aluminum honeycomb crushing force gradually decreases with the temperature increases.The peak pressure,burning rate coefficient and velocity increase while the peak time decreases with the temperature increase for the interior ballistics.For the launcher recoil responses,the average launch recoil decreases if the aluminum honeycomb doesn't enter the dense stage.The impact acceleration,projectile velocity and displacement increase as the temperature increase.The paper spotlights the temperature's influence on the recoil characteristics of the aluminum honeycomb buffer,which provides a new idea for buffering technology of pyrotechnic devices in a complex space environment.

    1.Introduction

    The number of space debris increases with the development of human space activities [1].Space debris poses a serious threat to spacecraft safety and affects the launching of new satellites [2,3].Therefore,Active Debris Removal (ADR) techniques have attracted increasing attention from significant space agencies and academic communities all around the world [4].One is the stiff connection capture using robotic arms or tentacles [5];the other is flexible connection capture using tether-net or flying gripper[6].The latter allows the capture from a long distance between the target and the chaser spacecraft [7].Compared with other capture mechanisms for ADR,such a tether-net system has a lighter weight,smaller volume and higher compatibility with an unknown target's shape and dynamic characteristic because of its flexibility.Besides,the tether-net system can perform the capture at a safe distance from the space target and does not need relative attitude control at a high cost [8],and the tether-net technique becomes a research hotspot [9].

    Removing space debris using a tether-net system includes four phases: launch,contact,closing and pulling.The main launch methods of tether-net include spring ejection[10]and pyrotechnic launching [11].Pyrotechnic devices are widely used by the aerospace and defense industries [12].They provide high efficiency,high energy per unit weight,lighter weight,and controllable initiation and output energies [13,14].During the work of those pyrotechnic devices,a harsh mechanical environment known as pyroshock is inevitably induced by explosions with high frequency,short duration and high acceleration shock response,which could damage the nearby micro mechanism and hardware sensitive to high-frequency shock,and even cause disastrous flight accidents[15].Pyroshock rarely causes damage to structural members,and it can easily cause failures in electronic and optical components that are sensitive to high-frequency energy and failures in the relay and magnetic components that are sensitive to low frequency ranges from 2 to 4 kHz[16].Moening showed that 74% of the flight failures that occurred from 1963 to 1985 were highly suspected caused by pyroshock [17].Since 1960,the National Aeronautic and Space Administration (NASA) [18],European Space Agency (ESA) [19],Sandia National Laboratories (SNL) [20,21]and the United States Military (USM) [22]have performed many standards to guarantee the reliability of launching missions.The published kinds of literature on pyroshock have mainly focused on the modeling and experiments of different pyrotechnic devices and there are relatively few reports on pyroshock isolation [23,24].

    Honeycomb structures are extensively applied to engineering and various industries such as aviation,aerospace,and transportation as load and thermal-resistance barriers,the core of sandwich structures,and impact energy-absorbing structures due to superior mechanical properties and considerable loadingbearing advantages impact [25,26].Aluminum honeycomb can absorb kinetic energy from impact and delay or attenuate stress waves in a typical explosion [27,28].The environment that spacecraft work in outer is terrible due to the external temperature being up and down,which will cause a great test to the regular operation of the spacecraft.With radiation from other stars,spacecraft in space absorbs heat,causing temperature fluctuations.The temperature change has a great relationship with the orbit of the spacecraft.It will also cause the thermal response of the spacecraft's internal structure,equipment,deformation,vibration and other consequences to affect its regular operation during the life period.Therefore,it is necessary to consider the change in space temperature when reducing the impact of the launch of a pyrotechnical device on the satellite platform through a buffer.

    It innovatively introduced a buffer structure using an aluminum honeycomb to attenuate the pyroshock generated by the tether-net launcher in this paper.Firstly,the characteristics of aluminum honeycomb and gunpowder at different temperatures were obtained through experiments and simulations.Secondly,a recoil experiment was carried out to validate the numerical simulation.Finally,the temperature effects of the launcher with aluminum honeycomb buffer were analyzed.

    This paper is organized as follows.In Section 2,the structure and working process of the aluminum honeycomb buffer is discussed.The quasi-static compression experiments and simulations of aluminum honeycomb at different temperatures and the theory of the crushable foam plasticity model are presented in Section 3.Closed bomb tests and internal ballistic properties at different temperatures are researched in Section 4.Recoil simulation,verification experiment and launch characteristics at different temperatures are discussed in Section 5,and the conclusions are provided in Section 6.

    2.The structure and working process of the aluminum honeycomb buffer

    A new buffer structure was designed in this paper,as is shown in Fig.1 and Table 1.It mainly includes a chamber,an aluminum honeycomb buffer and an igniter.The gunpowder is placed between the chamber and the chamber cover.An aluminum honeycomb buffer is put between the top plate and bottom plate,and the bottom plate is tied to the launch frame.There are six throughholes in the top plate,and a sleeve is installed on each throughhole.The sleeves are fixed on the bottom plate through threads to limit the movement direction of the top plate and aluminum honeycomb.

    Fig.1.Buffer structure.

    Table 1 The material for the main parts.

    The igniter starts to work after receiving the signal.The igniter fires the gunpowder near the igniter.As the gunpowder continues to burn,a large amount of high-temperature and high-pressure gas will be produced,which works on the projectile bottoms to push them moving.The gas also acts on the chamber and chamber cover generating the recoil.The projectiles will be made forward with kinetic energy and reach a certain velocity as they leave the canister.The chamber and chamber cover move downward,causing the top plate to go below.The launch platform will be significantly impacted if the recoil force is too large.Therefore,it is necessary to design a buffer structure between the launch device and the platform for absorbing excess energy to ensure a safe launch.

    The aluminum honeycomb begins to collapse when the downward movement of the top plate.The crushing deformation of the aluminum honeycomb absorbs the crushing force that exceeds the value of the aluminum honeycomb's steady-state collapse stage.Therefore,as the gunpowder continues to burn,the launch recoil force can be kept in a stable range,maximizing buffering and ensuring the launcher's and the platform's safety and reliability.

    3.The experiment and simulation of aluminum honeycomb at different temperatures

    In this section,the mechanical properties of aluminum honeycomb were obtained by quasi-static precompression tests at room temperature and complete crushing tests at different temperatures.The experimental results were used as input parameters of quasistatic simulation to verify the accuracy of the crushable foam plasticity model.

    3.1. Quasi-static compression experiments of aluminum honeycomb

    According to the mission requirements,the satellite platform will not be affected when the launch recoil is less than 21 kN.As shown in Fig.2,The specimen shape is cirque,with an outer diameter of 184 mm and an inner diameter of 148 mm;the crosssectional area is 8867 mm2.So the plane compression strength is 2.37 MPa.According to the“HB5443-1990 Specification for Durable Aluminium Honeycomb Core Materials for Sandwich Structures”,the aluminum foil material is 3003,with a foil thickness is 0.05 mm.The nominal length and density of aluminum honeycomb cells processed by aluminum foil are 2 mm and 105 kg/m3,respectively.

    Fig.2.Dimension of aluminum honeycomb.

    The quasi-static compression experiment using ETM series electromechanical universal testing machines was carried out to study the mechanical properties of aluminum honeycomb.The plate compressed the aluminum honeycomb at a 2 mm/min speed.The displacement-load curve acquired through quasi-static compression is shown in Fig.3(a).According to the result,the curve can be divided into four parts: A-B is the elastic stage.The elastic deformation of aluminum honeycomb occurs,and the relationship between displacement and load is linearly proportional.B-C is the dynamic buckling stage;C-D is the steady-state collapse stage,the aluminum honeycomb's primary energy absorption stage.As the displacement increases,the load almost remains unchanged.D-E is the dense stage,and the whole quasistatic compression process ends when the aluminum honeycomb enters the dense stage [29,30].

    Fig.3.Displacement load curves: (a) Complete compression;(b) Precompression and complete compression.

    The aluminum honeycomb is precompressed for 3 mm to maintain stable energy absorption during the compression energy absorption process,eliminating the B-C dynamic buckling stage,as shown in Fig.3(b).When the precompression aluminum honeycomb is compressed again,the displacement-load curve will be directly transferred from the elastic stage to the steady-state collapse stage,ensuring the stability of the energy absorption effect.

    The quasi-static compression experiments were carried out at +40,+30,+20,+10,0,-10,-20 and -30°C to study the temperature effects of the aluminum honeycomb,with three aluminum honeycomb specimens at each temperature.Firstly,the twenty-four aluminum honeycomb specimens were precompressed at quasi-static room temperature(about+10°C),and then the aluminum honeycomb specimens were completely compressed at corresponding temperatures.The specimens were heated in an oven and cooled with liquid nitrogen.Experiment types of equipment are shown in Fig.4.

    Fig.4.The types of experiment equipment at different temperatures: (a) High temperature;(b) Low temperature.

    The quasi-static experiment results at different temperatures are shown in Fig.5.In the displacement-load curves,‘1′represents the precompression curve of 1#aluminum honeycomb specimen at room temperature,and‘1-1′represents the complete compression curve of 1# aluminum honeycomb specimen at the room temperature.It is clear that the curves of‘3-1′at+40°C,‘3-1′at-10°C and‘1-1′at-30°C are different from the others;the curves are short in the steady-state collapse stage.The reason is that the aluminum honeycomb specimens were squished during the experiments.When one side of the specimen enters the dense stage,the other side is still in the steady-state collapse stage,as shown in Fig.6.Therefore,the curves are invalid,and the data must be removed.

    Fig.5.Aluminum honeycomb experiment results: (a) +40 °C;(b) +30 °C;(c) +20 °C;(d) +10 °C;(e) 0 °C;(f) -10 °C;(g) -20 °C;(h) -30 °C.

    Fig.6.Invalid aluminum honeycomb specimen.

    As is shown in Fig.6,taking +40°C.as an example.At room temperature,‘1′,‘2′and ‘3′are the precompression curves of aluminum honeycomb specimens.Each specimen was crushed by 3 mm to eliminate the dynamic buckling stage.‘1-1′,‘2-1′and‘3-1′are the complete compression curves of specimens at +40°C.By comparing the displacement-load curves of each specimen,it can be found that there is a longer displacement in the elastic stage after being precompressed.The reason is that when the aluminum honeycomb specimen is precompressed,the crushed side of the specimen is destroyed.When the specimen is crushed again,the damaged side continues to be crushed and destroyed.However,it doesn't need to go through the dynamic buckling stage,directly from the elastic stage to the steady-state collapse stage,and finally to the dense section to complete the collapse.

    The statistical results of the tests are shown in Table 2.It can be seen that as the temperature increases,the crushing force of aluminum honeycomb specimens gradually decreases.Compared with room temperature,the average force reduces by 13.06% at +40°C and increases by 8.55% at -30°C.There are two main reasons:aluminum foil and organic adhesives.The yield strength of aluminum foil material decreases with the temperature increases.The J71 adhesive developed by Heilongjiang Petrochemical Research Institute is used to prepare aluminum honeycomb.After curing,the adhesive is resin material,softened at high and hardened at low temperatures [31].The common and consistent changes in the strength of aluminum foil and binder at different temperatures eventually change the strength of the honeycomb with temperature.

    Table 2 Statistical table of experiment results.

    3.2. The simulation of aluminum honeycomb quasi-static compression

    3.2.1.The theory of the crushable foam plasticity model

    ABAQUS's crushable foam plasticity model for analyzing crushable foams is typically used in energy absorption structures.Two phenomenological constitutive models are presented: the volumetric hardening and isotropic hardening models.Both models use a yield surface with an elliptical dependence of deviatory stress on pressure stress in the meridional plane [32].

    The isotropic hardening model assumes symmetric behavior in tension and compression.The yield surface evolution is governed by an equivalent plastic strain,contributing to the volumetric and deviatory plastic strain.Therefore,the isotropic hardening model is adopted in this paper.

    The isotropic hardening model was initially developed for metallic foams.The model assumes similar behaviors in tension and compression.The yield surface is an ellipse centered at the origin in thep-q stress plane and evolves in a self-similar manner governed by the equivalent plastic strain [32].

    The yield surface for the isotropic hardening model is defined as

    where α represents the shape of the yield ellipse in thep-q stress plane,and B defines the size of the yield strength in uniaxial compression.The yield surface is the Mises circle in the deviatory stress plane and an ellipse in the meridional plane,as depicted in Fig.7.

    Fig.7.Yield surfaces and flow potential for the isotropic hardening model [32].

    The parameter α can be calculated using the initial yield stress in uniaxial compressionand the initial yield stress in hydrostatic compression,as

    The strength ratiokmust be in the range of 0 and 3.For many low-density foams,the initial yield surface is close to a circle in thep-qstress plane,which indicates that the value of α is approximately one.The special case ofk=0 corresponds to the Mises yield surface.

    The flow potential for the isotropic hardening model is chosen as

    where β represents the shape of the flow potential in the p-q stress plane and is related to the plastic Poisson's ratio vp,by

    The plastic Poisson's ratio,which is the ratio of the transverse to the longitudinal plastic strain under uniaxial compression,should be defined by the user;and it must be in the range of -1 and 0.5.The upper limitvp=0.5 corresponds to an incompressible plastic flow[33].

    The plastic flow is associative when the value of β is the same as that of α.In general,the plastic flow does not associate with allowing for the independent calibrations of the yield surface shape and the plastic Poisson's ratio.For many low-density foams,the plastic Poisson's ratio is nearly zero,corresponding to a value of β=2.12 [34].

    When α and β are identical,the plastic flow is correlated.By default,the plastic flow is uncorrelated,allowing the yield surface.Furthermore,the plastic Poisson's ratio is calibrated independently of each other.Suppose only the value of plastic Poisson's ratio vpis obtained.In that case,the relevant plastic flow can be selected,and the compression yield stress ratio k can be calculated according to the plastic Poisson's ratio vp

    A simple uniaxial compression test is sufficient to define the evolution of the yield surface.The hardening law defines the yield stress value in uniaxial compression as a function of the absolute value of the axial plastic strain.

    The engineering strain-stress curve of the aluminum honeycomb can be obtained from the displacement-load curve obtained by the above axial compression experiment.The engineering strain εengand the engineering stress σengare defined as follows:

    whereFis the tension or pressure exerted on a specimen at the moment,A0is the initial sectional area of the specimen,lis the instantaneous distance length after deformation,andl0is the initial length.Engineering strain and stress have positive and negative differences.

    The cross-section area used for engineering stress is the cross in the state of no stress before experimental loading.However,in the actual loading process,axial deformation of materials is accompanied by transverse deformation,resulting in changes in the real cross-section during loading.True stress σtruerefers to the true stress during loading,which is derived from the force and true section

    whereAtrueis the instantaneous cross-section area at a certain time during loading.

    The true stress cannot be directly measured experimentally but is usually calculated by a series of assumptions.For most foam materials,the plastic Poisson's ratio is generally 0,and the transverse deformation is minimal in the compression process.It can usually be considered that the cross-section area of foam materials does not change during compression.Therefore,for foam materials,true stress is equal to engineering stress.The instantaneous lengthlof the specimen in the tensile process was differentiated,and the true strain increment dεtrueat a certain moment was obtained as follows:

    The true strain can be obtained by integrating the above equation εtrue

    Therefore,the relationship between the true strain and engineering strain can be obtained

    The true stress-strain curves of aluminum honeycomb can be obtained by smoothing the true stress and strain data,and the main material properties of aluminum honeycomb is shown in Table 3.

    Table 3 Material properties of aluminum honeycomb.

    3.2.2.The simulation model

    A simulation model was established according to the aluminum honeycomb quasi-static compression experiment,as shown in Fig.8.The plate and base deformation during the quasi-static compression process is minimal and can be ignored.So they are regarded as rigid bodies,and the aluminum honeycomb adopts the plastic crushable foam model.And the details of the finite element model are shown in Table 4.The base was fixed.The plate could only move down on theZ-axis at a certain speed of 100 mm/s.

    Fig.8.Simulation model.

    Table 4 Main parameters of the finite element model.

    The displacement-load curves of the aluminum honeycomb in the simulation are shown in Fig.9.It can be seen that the displacement-load curves of the simulation and experiment are consistent.Different aluminum honeycomb crushing force peaks are distant in the same experimental conditions.Therefore,the simulation accuracy must be judged by the steady-state collapse part in the simulation and experiment displacement-load curves.In the steady-state collapse stage (displacement in 3-10 mm),the average value of the experiment collapse force is 20.044 kN.The average simulation value is 19.978 kN,and the error is 0.33% compared with the experiment.

    Fig.9.Experiment and simulation displacement-load curves.

    3.3. The simulation and test results

    Simulation and test results of aluminum honeycomb specimens at different temperatures are shown in Fig.10,and the statistical data of the simulation and test results are shown in Table 5.At each temperature,the displacement-load curves of aluminum honeycomb specimens directly transition from the elastic stage to the steady-state collapse stage and finally to the dense section,showing the same trend.Through data statistics,the maximum and minimum error of the experiment and simulation crushing force at different temperatures is 0.46% and 0.02% in the steady-state,and the total average error is 0.255%,proving the correctness of the plastic crushing foam model and the quasi-static crushing simulation model.

    Fig.10.Experimental and simulation results: (a) +40 °C;(b) +30 °C;(c) +20 °C;(d) +10 °C;(e) 0 °C;(f) -10 °C;(g) -20 °C;(h) -30 °C.

    Table 5 Statistical table of test and simulation results.

    4.The interior ballistic properties of the pyrotechnic device at different temperatures

    In this section,the powder power and burning rate coefficient of gunpowder were obtained by closed bomb tests at different temperatures,which were used as the input parameters of the internal ballistic model to get the properties of the pyrotechnic device.

    4.1. The closed bomb tests

    In internal ballistic experiments,closed bomb devices are often used to study gunpowder's combustion and gas formation under constant volume conditions [35].Two critical data are obtained from the closed bomb test: peak pressure and peak time.The powder power and burning rate coefficient in the burning rate equation of gunpowder can be gained,which can be used for internal ballistic analysis.

    In a closed bomb device,excluding heat loss,according to the first law of thermodynamics [36].

    where dQis the change in heat energy into the working volume,dEis the change in energy in the gas,andpdWis the change in energy of work done by gas expansion.

    Under the condition of constant volume,the volume of gunpowder is tiny,andpdWcan be ignored,then Eq.(13) can be changed into

    During the combustion of gunpowder,the mass of gas ωg=ωψ increases.Therefore,the heat is increasing

    where ω is the mass of gunpowder charge,ψ is the mass fraction of gunpowder burned off,ωgis the mass of charge in the gas phase of gunpowder combustion,and QWis the explosive heat of gunpowder.

    Under the condition of constant volume,the gaseous inner energy is expressed as

    Introduce specific heat ratiok=cp/cv,and consider the Mayer equation:

    wherecpis the specific heat of gunpowder at constant pressure,cVis the specific heat of gunpowder at constant volume,Tis temperature,Ris the gas constant;α=1×10-3m3·kg-1is co-volume,pis pressure,and θ=k-1 is the thermal coefficient.Eqs.(15) and(20) can be obtained simultaneously

    wheref=RT1is powder power.

    When the mass combustion ratio of gunpowder is ψ,pψ=p,Wψ=W,

    whereWψis the free volume of the chamber,andW0is the initial volume of the chamber.

    Before the gunpowder burns,i.e.ψ=0,Wψ=W0-ω/δ;and when the gunpowder is finished burning,i.e.ψ=1,Wψ=W0-αω.According to Eq.(23),the maximum pressurepmmunder constant volume condition occurs at the moment when the gunpowder combustion ends,

    Make the packing density Δ=ω/W0,

    The closed bomb tests were carried out at+40,+10 and-30°C to study the gunpowder properties at different temperatures.And three tests were performed at each temperature to avoid the experiment's randomness.The structure of the closed bomb in this study is shown in Fig.11;one section of the cylinder is screwed into the igniter plug 2,which relies on an electric current to gunpowder 3,thus causing gunpowder 4 to burn.The pressure produced by gunpowder combustion and its time-varying law is recorded by the pressure sensor 5 screwed into the other end and various recording instruments.In this test,the chamber volume is 530 mL,and the mass of gunpowder 4 is 7.3 g.

    Fig.11.Structure of closed bomb.

    Fig.12.+40 °C: (a) 1#;(b) 2#;(c) 3#.

    Fig.13.+10 °C: (a) 1#;(b) 2#;(c) 3#.

    The internal ballistic equations under a constant volume state were established to obtain the two key parameters: gunpowder powder power and burning rate coefficient.The results of tests and simulations are shown in Figs.12-14.It can be seen from the pressure curves that the simulation results are in good agreement with the test results.The pressure curves at different temperatures increase from zero until it remains stable.In the constant volume,at the initial ignition stage,the chamber pressure rises gradually with the combustion of the gunpowder.When the gunpowder gas is filled with the container,the chamber pressure will remain stable with the gunpowder's continued combustion until the burst is completed.

    To better match the pressure curves of the test and simulation,it is necessary to offset the simulated pressure curve in time to ensure the accuracy of the internal ballistic parameters.The initial chamber pressure doesn't affect the peak pressure and peak time,so the error is negligible.

    The peak pressure,burning rate coefficient and powder power at different temperatures are shown in Table 6 according to the tests and the solution of the constant volume internal ballistic equation.And in the table,Pemrepresents the experiment peak chamber pressure,Psmrepresents the simulation peak chamber pressure andu1represents the burning rate coefficient.Compared with the experimental results,the maximum error of peak pressure simulation is 2.42%,and the minimum error is 0%,proving the accuracy of internal ballistic simulation at different temperatures under constant volume.

    Table 6 Table of test and simulation results of closed explosive.

    Eq.(26)can solve the powder powerf.Therefore,it can be seen that the powder power is only related to the peak pressurePmand the burning rate coefficientu1obtained through the test data optimization.Moreover,the peak pressurePmand the burning rate coefficientu1increase gradually with the temperature increase.The powder powerfrefers to the power of gunpowder per unit mass,so the higher the powder power,the higher the peak pressure.The burning rate coefficientu1represents the speed of combustion of gunpowder.The larger the burning rate coefficient,the faster the gunpowder combustion rate is and the shorter the peak pressure time.It can be seen from Figs.12-14 that the average time to peak pressure of gunpowder chamber pressure at+40°C is the shortest,which is about 2.28 ms,the time is about 3 ms at +10°C,and the longest time is approximately 3.40 ms at -30°C.

    Figs.14.-30 °C: (a) 1#;(b) 2#;(c) 3#.

    In conclusion,as the temperature increases,gunpowder's peak pressure and burning rate coefficient increase while the peak time decreases.

    4.2. Internal ballistic properties at different temperatures

    Studying the launcher's interior ballistic is necessary to obtain its recoil force.The six launch canisters share the same chamber.According to the parameter equivalence rule,the projectile's total mass is equivalent to the sum of the mass of six projectiles.The total cross-sectional area of the launch canister is equal to the sum of the cross-sectional area of six launch canisters.

    Each projectile is symmetrically fixed in the launch canister by two copper pins with a diameter of 2.6 mm,and the shear strength of a copper pin is 300 MPa.Thus,the shear force of a single copper pin is 1600 N,and the total shear force of a single launch canister is 3200 N.The shear force can be converted into the projectile starting pressureP0=3.52 MPa.

    The interior ballistic properties of the launcher can be acquired by the equivalent launch model adopting the classical internal ballistic equation,which is as follows [37,38]:

    For the above internal ballistic equation,the main calculation parameters are shown in Table 7,and the results of the internal ballistic at +10°C are demonstrated in Fig.15.The duration of the chamber pressure of the launcher is 6.09 ms,and the maximum chamber pressurePmis 8.67 MPa.

    Fig.15.Interior ballistics curves: (a) Chamber pressure curves;(b) Displacement and velocity curves.

    When the pressure produced by gunpowder in the chamber doesn't meet the starting chamber pressure,the projectiles stay still,as is shown in stages A-C in Fig.15(a).In stage C-Pm,the projectiles move after the pressure exceeds the starting chamber pressure.The influence of the rate of gunpowder gas generation on chamber pressure is greater than that of the growth of space volume after projectile motion,and the pressure curve keeps rising.When these two influences reach balance,chamber pressure reaches the maximum.In stages Pm-D,with the continuous increase of the projectile velocity,the influence of the rise of the space volume after the projectile movement exceeds the effect of the gas generation rate,and the chamber pressure begins to decline.When the powder burns completely,the chamber pressure decreases with the increases in the velocity of the projectiles.

    As described earlier,a single projectile is fixed by copper pins before firing,and only when the chamber pressure exceeds the shear strength of the copper pins (i.e.,the starting chamber pressure) does the projectile begins to move.Thus,the chamber pressure loaded on the projectile is divided into A-B-C and C-D.

    As shown in Fig.15(b),the projectile's distance away from the launcher canister is 55 mm,and the projectile's velocity is 22.25 m/s.The displacement and velocity of the projectile are zero for about 2 ms at the beginning.The reason is that the chamber pressure has not reached the starting chamber pressure.When the pressure exceeds the starting chamber pressure,the projectile moves until it leaves the launch canister.

    The interior ballistic curves at different temperatures are shown in Fig.16.It can be seen that the peak chamber pressure and the projectile launch velocity increase with the temperature increase,but the peak time and projectile flight time are reduced.The reason is that with the temperature increase,the peak pressure,burning rate coefficient and powder power of gunpowder increase.

    Fig.16.Interior ballistics curves at different temperatures: (a) Chamber pressure curves;(b) Velocity curves;(c) Displacement curves.

    5.The recoil simulation and experiment

    In this section,based on the aluminum honeycomb and interior ballistic characteristics at different temperatures,the recoil model of the tether-net launcher was established,which was verified by the experiment,.and the recoil performance of the launcher at different temperatures was analyzed.

    5.1. Recoil simulation and verification experiment

    The dynamic launch model was built in ABAQUS/EXPLICIT.The launch frame is fixed,and because the rest of the parts have a more negligible effect on the launch recoil force,the aluminum honeycomb components are set to the rigid body to speed up the calculation.

    In the quasi-static test,the initial height of the aluminum honeycomb specimen is 12 mm,the height after compression is 2 mm,and the loading speed is 2 mm/min,so the strain rate of the quasistatic test is 0.0028 s-1.In the launch recoil test,the initial height of the aluminum honeycomb is about 9 mm,the average height after compression is 5.133 mm,and the duration is about 6 ms,so the strain rate in the dynamic test is 71 s-1.

    According to the law of conservation of energy and the principle of minimum energy,obtained quasi-static mean plastic collapse stress under the Tresca yield criterion [39].

    where σ0is the yield stress of aluminum honeycomb material,tis aluminum honeycomb cell thickness,andlis cell length.

    The cross-sectional area of the specimen is 8867 mm2,and the collapse force is 21 kN,so the plane compression strength σm=2.37 MPa.To incorporate the strain rate effect of materials into the Cowper-Symonds,the formula of dynamic compressive plateau stress can be written as

    whereDandpare the strain rate material constants,for Al3003[40],D=24295.5 s-1,andp=1.094,the average height after compression is 5.133 mm,and the duration is about 6 ms,v=0.8555 m/s.

    Meanwhile,a recoil experiment was designed to verify the accuracy of the launch recoil simulation.The experiment layout is shown in Fig.17.

    The experiment and simulation process are shown in Fig.18.It can be seen that the experiment and simulation launch process are almost consistent.After the powder is ignited,there is a large amount of high-temperature and high-pressure gas.When the chamber pressure reaches the starting pressure,the copper pin is cut off,and the projectile moves along the launch canisters.After about 6 ms,the projectiles leave away from the launch canisters.The condition of the aluminum honeycomb before and after the experiment is shown in Fig.19.

    Fig.18.Experiment and simulation process: (a) t=0 ms;(b) t=2 ms;(c) t=4 ms;(d) t=6 ms;(e) t=6.5 ms;(f) t=10 ms.

    Fig.19.Aluminum honeycomb condition: (a) Before the experiment;(b) After the experiment.

    The projectile's velocity is 21.75 m/s,measured by the experiment.As shown in Fig.20,the projectile's displacement in interior ballistic and simulation is 55 mm and 60.8 mm simultaneously.And the velocity of the projectile in interior ballistic and simulation is 22.25 m/s and 23.849 m/s.So the interior ballistic velocity and simulation velocity errors are 2.3% and 9.65% compared with the experiment.The main reason is that there is a sealing ring between the projectile and the canister in the experiment.The sealing ring and the launch canister will produce greater friction to hinder the projectile's movement,leading to the experiment speed being less than the calculation and simulation speed of the interior ballistic.Moreover,the projectiles have a different displacements simultaneously because of the velocity error.

    The recoil curves of the experiment and simulation are shown in Fig.21.The peak recoil force of the experiment and simulation is 24.1328 kN and 18.962 kN.For the steady-state collapse stage(≥15 kN),the experiment and simulation average recoil forces are 19.552 kN and 18.66 kN.Compared with the experiment,the peak recoil error of the simulation is 21.4%,and the average recoil error is 4.56%.

    Fig.21.Recoil force comparison curves of experiment and simulation.

    As is shown in Fig.21,the recoil force curves of the experiment and simulation have little difference between the initial and end,mainly because the chamber pressure obtained by the interior ballistic model is the average chamber pressure,which has an inevitable error with the actual chamber pressure.

    In the experiment,recoil force presented two trends in the steady-state collapse stage and the first was the downward oscillation in the first half and the upward oscillation in the second half.It was mainly because with the increase of chamber pressure,the recoil speed of the chamber began to increase,leading to the rise of aluminum honeycomb collapse force.Therefore,in the dynamic launch simulation,the recoil force remains constant in the steadystate collapse stage,which is different from the oscillation phenomenon in the experiment.But these differences accounted for only 4.56% of the average recoil,so they were considered reasonable.

    In general,the simulation results match the experiment results in trends and magnitudes,validating the accuracy and reliability of the dynamic model.This provides a solid foundation for the following parameter analysis of deploying performance.

    5.2. The launch characteristics at different temperatures

    To explore the influence of different temperatures on the tethernet launcher's recoil force and emission characteristics,the launch dynamics simulation at +40,+10 and -30°C was set up.Fig.18 shows the launching characteristics at different temperatures,and Table 8 lists the critical parameters in the simulation results.

    Table 8 Statistical table of simulation results.

    The recoil curve can be divided into three stages for launch recoil: the rising stage,the stable stage,and the falling stage,respectively.In the increasing stage,+40°C firstly rises to the stable phase,and -30°C finally rises to the stable stage.As the temperature decreases,the burning rate and powder power decrease,resulting in a long time for chamber pressure to reach the honeycomb chamber pressure.In the stable stage,as shown in Table 8,the average force increases with the decrease in temperature,mainly because the aluminum honeycomb will soften at high and harden at low temperatures.

    For maximum recoil,the biggest is at+40°C,and the temperatures are more significant than the other.The reason is mainly due to the enhanced performance of gunpowder at +40°C resulting in more impulse and the softening of aluminum honeycomb,leading to the aluminum honeycomb in the compression process quickly into the dense stage,making a secondary increase in recoil force.At the temperature of +10°C and -30°C,the aluminum honeycomb doesn't enter the dense stage,so the difference between the average and maximum recoil force at these two temperatures is small.And because of the relationship between powder power and aluminum honeycomb crushing force with temperature,the lower the temperature,the shorter the recoil stability stage duration.In conclusion,under the premise that aluminum honeycomb doesn't enter the dense phase during the launching process,the average recoil decreases with the temperature increase.

    As for the impact acceleration,as shown in Fig.22(b) and Table 8,the maximum impact acceleration reaches 5651.9 g at +40°C,which is much higher than the other temperatures,mainly because the aluminum honeycomb enters the dense stage at this temperature and the recoil increases significantly.With the temperature decrease,the impulse produced by gunpowder decreases,and the crushing force of the aluminum honeycomb rises so that the aluminum honeycomb at the other two temperatures doesn't enter the dense stage,so the impact acceleration gradually decreases.To sum up,the impact acceleration produced by the tether-net launcher gradually increases with the temperature increase.

    Fig.22.Launching characteristics at different temperatures: (a) Recoil force curves;(b) Acceleration curves;(c) Velocity curves;(d) Displacement curves.

    As shown in Fig.22(c),the curve can be divided into the rising and stable stages for projectile launch velocity.In the rising phase,as the powder power and burning rate coefficient increase with the temperature increase,the time for chamber pressure to reach the starting chamber pressure becomes shorter.Hence,the projectile starts to move at +40°C firstly.As the powder continues to burn,the velocity of the projectile increases,and when it leaves the canister and keeps steady.As shown in Table 8,the projectile's speed fells by 2.12 m/s from the maximum to the final at +40°C.This is mainly because the aluminum honeycomb quickly reaches into the dense phase,increasing the chamber recoil displacement and velocity,leading to the projectile producing the opposite direction speed before it leaves the canister,which slows down the projectile velocity.At the other two temperatures,the aluminum honeycomb didn't enter the dense stage,so the maximum and final velocity of the projectile varied little.At the same time,it can also be seen that on the premise that the aluminum honeycomb doesn't enter the dense stage,the launch velocity of the projectiles increases with the temperature increases.

    As for the projectile displacement curve,as shown in Fig.22(d),the projectile's displacement also decreased due to the projectile velocity decrease at +40°C,while the projectile displacement remained stable at the other two temperatures.If the aluminum honeycomb doesn't enter the dense stage,the projectile displacement will gradually increase with increasing temperature.

    To sum up,with the temperature increases,the average launch recoil of the tether-net launcher decreases when the aluminum honeycomb doesn't enter the dense stage.However,the impact acceleration,projectile velocity and displacement will increase.

    6.Conclusions

    This paper designed a new buffer structure for the tether-net launcher to attenuate the large recoil force and impact.The characteristics of aluminum honeycomb and gunpowder at different temperatures were obtained through experiments and simulations.Based on the above data,the launching process was simulated with ABAQUS/EXPLICIT.In addition,the temperature effects on the tether-net launcher's recoil force and emission characteristics were analyzed.Some conclusions can be drawn as follows:

    (1) As the temperature increases,the crushing force of the aluminum honeycomb gradually decreases.Compared with force at+10°C,the average force reduces by 13.06% at+40°C and increases by 8.55% at -30°C.

    (2) Compared with responses at +10°C,when the temperature is +40°C,the average burning rate coefficient increase by 29.08%,the peak pressure increases by 6.9%,and the final velocity increase by 2.33%.When the temperature is-30°C,the average burning rate coefficient,the peak pressure and the final velocity decrease by 13.38%,6.44% and 2.43%,respectively.

    (3) Under the assumption that the aluminum honeycomb does not enter the dense stage with increasing temperature,the average recoil force would decrease by 3.82% at +40°C and increase by 11.69% at -30°C compared with +10°C.With temperature increases,the impact acceleration,projectile velocity and displacement will increase.

    Declaration of competing interest

    The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

    Acknowledgments

    This work was supported by the National Natural Science Foundation of China (Grant No.52102436);the Fundamental Research Funds for the Central Universities (Grant No.30920021109);Natural Science Foundation of Jiangsu Province(BK20200496);China Postdoctoral Science Foundation (Grant No.2020M681615);the project of Key Laboratory of Impact and Safety Engineering (Ningbo University),Ministry of Education (Grant No.CJ202107);and the State Key Laboratory of Mechanics and Control of Mechanical Structures (Nanjing University of Aeronautics and astronautics) (Grant No.MCMS-E-0221Y01).

    男女边摸边吃奶| 日日啪夜夜爽| 蜜桃久久精品国产亚洲av| 国产精品一二三区在线看| 久久影院123| 精品国产一区二区久久| 最近最新中文字幕免费大全7| 欧美日韩视频精品一区| 久久国产乱子免费精品| 亚洲av中文av极速乱| 色网站视频免费| 永久免费av网站大全| 在线观看av片永久免费下载| 日本色播在线视频| 免费大片18禁| 一本大道久久a久久精品| 在线亚洲精品国产二区图片欧美 | 国产成人免费观看mmmm| 色吧在线观看| 午夜激情久久久久久久| 天堂8中文在线网| 99久久综合免费| 美女cb高潮喷水在线观看| av女优亚洲男人天堂| a 毛片基地| 一级av片app| 中文在线观看免费www的网站| 乱人伦中国视频| 夜夜骑夜夜射夜夜干| 最近手机中文字幕大全| 丝袜在线中文字幕| 午夜影院在线不卡| 国内精品宾馆在线| 午夜老司机福利剧场| av福利片在线| 亚洲av.av天堂| 亚洲怡红院男人天堂| 免费不卡的大黄色大毛片视频在线观看| 国产亚洲最大av| 啦啦啦中文免费视频观看日本| 精品少妇内射三级| 国产亚洲欧美精品永久| 亚洲国产欧美在线一区| 毛片一级片免费看久久久久| 黄色视频在线播放观看不卡| 极品少妇高潮喷水抽搐| 日韩欧美一区视频在线观看 | 国产精品一区二区在线不卡| 国产精品国产三级国产专区5o| 免费看av在线观看网站| 久热这里只有精品99| 久久人妻熟女aⅴ| 国产精品偷伦视频观看了| 七月丁香在线播放| 啦啦啦中文免费视频观看日本| 午夜福利影视在线免费观看| 亚洲国产精品国产精品| 水蜜桃什么品种好| 免费高清在线观看视频在线观看| 69精品国产乱码久久久| 一级片'在线观看视频| 久久ye,这里只有精品| 日日爽夜夜爽网站| 99久久精品国产国产毛片| 国产无遮挡羞羞视频在线观看| 欧美日韩亚洲高清精品| 少妇的逼水好多| 三级经典国产精品| 国产 一区精品| 最近最新中文字幕免费大全7| 人人澡人人妻人| 国语对白做爰xxxⅹ性视频网站| 99热全是精品| 国产深夜福利视频在线观看| 久久狼人影院| 少妇精品久久久久久久| 99re6热这里在线精品视频| 久久这里有精品视频免费| 亚洲精华国产精华液的使用体验| 欧美区成人在线视频| 日韩人妻高清精品专区| www.色视频.com| 免费观看性生交大片5| 国产淫片久久久久久久久| 欧美日韩亚洲高清精品| 最近中文字幕2019免费版| 免费人妻精品一区二区三区视频| 久久青草综合色| 一本一本综合久久| 国产午夜精品一二区理论片| 国产成人精品久久久久久| 国产黄频视频在线观看| 精品少妇久久久久久888优播| 曰老女人黄片| 夜夜爽夜夜爽视频| h日本视频在线播放| 亚洲第一区二区三区不卡| 欧美日韩精品成人综合77777| 在线观看国产h片| 美女cb高潮喷水在线观看| 国产乱来视频区| 蜜桃在线观看..| 欧美三级亚洲精品| 国产成人91sexporn| 能在线免费看毛片的网站| 欧美成人精品欧美一级黄| 青春草视频在线免费观看| 久久毛片免费看一区二区三区| 九草在线视频观看| 日韩不卡一区二区三区视频在线| 久久精品久久精品一区二区三区| 免费看av在线观看网站| 午夜视频国产福利| 国产一区二区三区av在线| 少妇的逼好多水| 欧美日韩国产mv在线观看视频| 亚洲国产精品成人久久小说| 精品亚洲乱码少妇综合久久| 国产成人精品久久久久久| 国产一区二区在线观看av| 免费久久久久久久精品成人欧美视频 | 国产真实伦视频高清在线观看| 亚洲国产欧美在线一区| 国内精品宾馆在线| 一级爰片在线观看| 91精品一卡2卡3卡4卡| 日韩一本色道免费dvd| 国产成人91sexporn| 一二三四中文在线观看免费高清| 晚上一个人看的免费电影| 亚洲成色77777| 欧美日韩视频精品一区| 久久久久久久精品精品| 久久精品国产亚洲网站| 丁香六月天网| 亚洲欧美精品自产自拍| 亚洲精品色激情综合| 男男h啪啪无遮挡| 亚洲人与动物交配视频| 日韩欧美一区视频在线观看 | 热99国产精品久久久久久7| 国产成人精品一,二区| 亚洲中文av在线| 国产熟女午夜一区二区三区 | 在线观看美女被高潮喷水网站| 水蜜桃什么品种好| 18+在线观看网站| 日产精品乱码卡一卡2卡三| 久久久久国产精品人妻一区二区| 中文字幕亚洲精品专区| 大陆偷拍与自拍| 十分钟在线观看高清视频www | 亚洲av在线观看美女高潮| 伊人久久精品亚洲午夜| 国内揄拍国产精品人妻在线| 日韩 亚洲 欧美在线| 亚洲第一av免费看| 国产精品久久久久久久电影| 日本wwww免费看| 18禁在线播放成人免费| 国产乱来视频区| 久久久欧美国产精品| 中文字幕人妻丝袜制服| 免费不卡的大黄色大毛片视频在线观看| 久久国产亚洲av麻豆专区| 天堂俺去俺来也www色官网| 成人午夜精彩视频在线观看| 亚洲av欧美aⅴ国产| 国产真实伦视频高清在线观看| 亚洲国产精品一区三区| 亚洲av综合色区一区| 岛国毛片在线播放| 黑人高潮一二区| videossex国产| 亚洲成人一二三区av| www.av在线官网国产| 自拍偷自拍亚洲精品老妇| 亚洲av电影在线观看一区二区三区| 国产成人免费无遮挡视频| 香蕉精品网在线| 在线精品无人区一区二区三| 国产亚洲欧美精品永久| 秋霞在线观看毛片| 九九在线视频观看精品| 十分钟在线观看高清视频www | 成人美女网站在线观看视频| 色94色欧美一区二区| 久久久久精品久久久久真实原创| 亚洲欧美清纯卡通| av视频免费观看在线观看| 午夜日本视频在线| 久久国产乱子免费精品| 夜夜骑夜夜射夜夜干| 观看免费一级毛片| 自拍偷自拍亚洲精品老妇| 亚洲情色 制服丝袜| 人妻系列 视频| 免费看光身美女| 自拍偷自拍亚洲精品老妇| 丰满迷人的少妇在线观看| 三级国产精品片| 蜜桃在线观看..| 3wmmmm亚洲av在线观看| 男男h啪啪无遮挡| 高清毛片免费看| 永久网站在线| 午夜激情久久久久久久| 国产黄色视频一区二区在线观看| 性高湖久久久久久久久免费观看| 久久久久视频综合| 久久久久网色| 午夜福利,免费看| 亚洲天堂av无毛| 国产日韩一区二区三区精品不卡 | 免费av中文字幕在线| 美女视频免费永久观看网站| av天堂中文字幕网| 大片电影免费在线观看免费| 丝袜脚勾引网站| av有码第一页| 自拍欧美九色日韩亚洲蝌蚪91 | 亚洲精品中文字幕在线视频 | 一区二区三区精品91| 久久午夜综合久久蜜桃| 热re99久久精品国产66热6| 少妇的逼水好多| 欧美亚洲 丝袜 人妻 在线| 99九九线精品视频在线观看视频| 在线亚洲精品国产二区图片欧美 | 成人亚洲精品一区在线观看| 亚洲av男天堂| a 毛片基地| 少妇被粗大的猛进出69影院 | 精品人妻熟女av久视频| 久久狼人影院| 一区二区三区精品91| 综合色丁香网| av线在线观看网站| 寂寞人妻少妇视频99o| 18禁裸乳无遮挡动漫免费视频| 夜夜骑夜夜射夜夜干| 久久国产精品男人的天堂亚洲 | 亚洲精品中文字幕在线视频 | 两个人的视频大全免费| 日韩强制内射视频| 亚洲国产精品成人久久小说| 热99国产精品久久久久久7| 人妻 亚洲 视频| 制服丝袜香蕉在线| 少妇裸体淫交视频免费看高清| 亚洲av综合色区一区| 中国美白少妇内射xxxbb| 在线观看免费日韩欧美大片 | 一本—道久久a久久精品蜜桃钙片| 在现免费观看毛片| 亚洲人成网站在线观看播放| 大码成人一级视频| 久久99热6这里只有精品| 精品少妇黑人巨大在线播放| 精品午夜福利在线看| 少妇人妻精品综合一区二区| 成年女人在线观看亚洲视频| 国产女主播在线喷水免费视频网站| 成人影院久久| 熟妇人妻不卡中文字幕| 制服丝袜香蕉在线| 大片免费播放器 马上看| 国产高清三级在线| av福利片在线观看| 国精品久久久久久国模美| 高清在线视频一区二区三区| 国产欧美日韩一区二区三区在线 | av网站免费在线观看视频| 搡老乐熟女国产| 免费黄色在线免费观看| 久久久久久久久久成人| 18禁裸乳无遮挡动漫免费视频| 丝袜在线中文字幕| 美女大奶头黄色视频| 少妇的逼好多水| 免费黄网站久久成人精品| 国产熟女欧美一区二区| 久久99热这里只频精品6学生| 亚洲av在线观看美女高潮| 久久热精品热| 日日爽夜夜爽网站| 黄色欧美视频在线观看| 国产一区二区在线观看日韩| 亚洲精品成人av观看孕妇| 日韩熟女老妇一区二区性免费视频| 五月玫瑰六月丁香| 久久久国产欧美日韩av| 国产真实伦视频高清在线观看| 亚洲国产精品成人久久小说| 女人久久www免费人成看片| 18禁裸乳无遮挡动漫免费视频| 午夜精品国产一区二区电影| 亚洲精品aⅴ在线观看| 日韩中文字幕视频在线看片| 亚洲精品国产av蜜桃| 女人久久www免费人成看片| 国产高清国产精品国产三级| 中文字幕制服av| 成年美女黄网站色视频大全免费 | 国产男人的电影天堂91| 欧美丝袜亚洲另类| 国产永久视频网站| 国产在视频线精品| 99热这里只有是精品50| 国产极品粉嫩免费观看在线 | 日韩中文字幕视频在线看片| 青春草国产在线视频| a级片在线免费高清观看视频| 日本av免费视频播放| 国产美女午夜福利| 精品国产一区二区三区久久久樱花| 嫩草影院新地址| av在线app专区| 22中文网久久字幕| 热99国产精品久久久久久7| 91精品一卡2卡3卡4卡| 最新中文字幕久久久久| 妹子高潮喷水视频| 寂寞人妻少妇视频99o| 黄色怎么调成土黄色| 熟女av电影| 99久久中文字幕三级久久日本| 最近手机中文字幕大全| 久久久久久久久久人人人人人人| 久久久久人妻精品一区果冻| 午夜视频国产福利| 国产成人91sexporn| 如何舔出高潮| 蜜臀久久99精品久久宅男| 亚洲,一卡二卡三卡| 亚洲精品一二三| 又大又黄又爽视频免费| 国产日韩欧美视频二区| 最新的欧美精品一区二区| 欧美日韩国产mv在线观看视频| 欧美高清成人免费视频www| 少妇被粗大猛烈的视频| 少妇 在线观看| 夫妻性生交免费视频一级片| 久久午夜综合久久蜜桃| 中文字幕久久专区| 欧美日韩综合久久久久久| 国产日韩一区二区三区精品不卡 | 少妇猛男粗大的猛烈进出视频| 99热这里只有是精品50| 最黄视频免费看| 在线 av 中文字幕| 成人亚洲欧美一区二区av| 中国国产av一级| 免费黄频网站在线观看国产| 日本色播在线视频| av女优亚洲男人天堂| 色94色欧美一区二区| 狂野欧美激情性xxxx在线观看| 99久久人妻综合| 男人舔奶头视频| 国产免费视频播放在线视频| 国产精品人妻久久久久久| 色吧在线观看| 免费黄网站久久成人精品| 91久久精品电影网| 久久精品久久精品一区二区三区| h视频一区二区三区| av网站免费在线观看视频| 黄色毛片三级朝国网站 | 亚洲欧美日韩东京热| 一本—道久久a久久精品蜜桃钙片| 精品人妻熟女av久视频| 国产精品久久久久久久电影| 亚洲欧洲日产国产| 黑人巨大精品欧美一区二区蜜桃 | 国产亚洲91精品色在线| 国产精品一区www在线观看| 国产欧美亚洲国产| 亚洲国产精品一区三区| 国产色婷婷99| 少妇人妻一区二区三区视频| 久久久久网色| 久久久国产精品麻豆| 国产精品三级大全| 亚洲不卡免费看| 最新中文字幕久久久久| 妹子高潮喷水视频| 成人免费观看视频高清| 91精品国产国语对白视频| 另类亚洲欧美激情| 中国国产av一级| 亚洲av成人精品一区久久| 日韩三级伦理在线观看| 亚洲精品国产av蜜桃| 亚洲天堂av无毛| 最近的中文字幕免费完整| 伊人亚洲综合成人网| 日韩欧美精品免费久久| 高清视频免费观看一区二区| 亚洲精品乱久久久久久| 日日啪夜夜爽| 国产精品秋霞免费鲁丝片| 国产黄色视频一区二区在线观看| 三级国产精品欧美在线观看| 最近2019中文字幕mv第一页| 国产av精品麻豆| 在线观看免费高清a一片| 91精品一卡2卡3卡4卡| 大片电影免费在线观看免费| 久久青草综合色| 午夜免费男女啪啪视频观看| 日韩制服骚丝袜av| 观看免费一级毛片| 亚洲精品乱码久久久久久按摩| 最后的刺客免费高清国语| 精品国产露脸久久av麻豆| 嫩草影院新地址| 欧美97在线视频| 欧美另类一区| 国产伦在线观看视频一区| 又粗又硬又长又爽又黄的视频| 久久狼人影院| 国产一区亚洲一区在线观看| 一个人看视频在线观看www免费| 日韩中文字幕视频在线看片| av专区在线播放| 桃花免费在线播放| 极品少妇高潮喷水抽搐| 久久国产精品大桥未久av | 人人妻人人澡人人爽人人夜夜| 免费大片18禁| 久久鲁丝午夜福利片| 欧美少妇被猛烈插入视频| kizo精华| 色哟哟·www| 国产成人午夜福利电影在线观看| 久久国产精品大桥未久av | 在线观看免费视频网站a站| 寂寞人妻少妇视频99o| 一区二区三区四区激情视频| 日本91视频免费播放| 亚洲经典国产精华液单| 国产精品熟女久久久久浪| 在线观看一区二区三区激情| 国产精品久久久久久久电影| 人人妻人人澡人人看| 国语对白做爰xxxⅹ性视频网站| 国产亚洲最大av| 美女内射精品一级片tv| 欧美日韩亚洲高清精品| 国产色爽女视频免费观看| 成年美女黄网站色视频大全免费 | tube8黄色片| 精品人妻熟女毛片av久久网站| 亚洲一区二区三区欧美精品| 欧美精品国产亚洲| 亚洲婷婷狠狠爱综合网| 九草在线视频观看| 精品国产一区二区久久| 一本一本综合久久| 熟女电影av网| 亚洲欧美清纯卡通| 免费看光身美女| 免费av中文字幕在线| 熟妇人妻不卡中文字幕| 亚洲精品,欧美精品| 秋霞在线观看毛片| 一级,二级,三级黄色视频| 欧美 亚洲 国产 日韩一| 亚洲经典国产精华液单| 国产精品女同一区二区软件| 久久这里有精品视频免费| 国产精品国产三级国产av玫瑰| 18禁动态无遮挡网站| 如日韩欧美国产精品一区二区三区 | 免费av不卡在线播放| 免费观看性生交大片5| 精品少妇黑人巨大在线播放| 3wmmmm亚洲av在线观看| 亚洲欧美一区二区三区国产| 亚洲国产精品一区二区三区在线| 一区二区三区乱码不卡18| 99re6热这里在线精品视频| 国产成人精品婷婷| 天堂俺去俺来也www色官网| 亚洲久久久国产精品| 婷婷色麻豆天堂久久| 成人漫画全彩无遮挡| 国产日韩欧美视频二区| 成人亚洲精品一区在线观看| 如日韩欧美国产精品一区二区三区 | 制服丝袜香蕉在线| 国产视频首页在线观看| 天堂俺去俺来也www色官网| 深夜a级毛片| 久久久久精品性色| 成年人免费黄色播放视频 | 中文精品一卡2卡3卡4更新| 人妻少妇偷人精品九色| 欧美高清成人免费视频www| 免费播放大片免费观看视频在线观看| 亚洲精品第二区| .国产精品久久| 18禁在线播放成人免费| 亚洲第一av免费看| av网站免费在线观看视频| 亚洲,一卡二卡三卡| 亚洲精品乱码久久久v下载方式| 国产精品一区二区性色av| 一级二级三级毛片免费看| 丝袜喷水一区| 国产成人91sexporn| 高清在线视频一区二区三区| 最新中文字幕久久久久| 99热这里只有精品一区| 免费观看a级毛片全部| 少妇人妻精品综合一区二区| 91久久精品电影网| 欧美日韩av久久| 纵有疾风起免费观看全集完整版| 婷婷色综合www| 夜夜看夜夜爽夜夜摸| 一二三四中文在线观看免费高清| h日本视频在线播放| 精品卡一卡二卡四卡免费| 熟女电影av网| 啦啦啦中文免费视频观看日本| 大又大粗又爽又黄少妇毛片口| 日韩中字成人| 久久99热6这里只有精品| 国产精品一区二区性色av| 亚洲av免费高清在线观看| 欧美+日韩+精品| 一级片'在线观看视频| 又爽又黄a免费视频| 国产熟女午夜一区二区三区 | 美女福利国产在线| 国产伦精品一区二区三区四那| av福利片在线| 51国产日韩欧美| 国产白丝娇喘喷水9色精品| 亚洲精品国产成人久久av| 另类亚洲欧美激情| 一边亲一边摸免费视频| 中文在线观看免费www的网站| 亚洲精品久久久久久婷婷小说| 国产成人免费观看mmmm| 国产精品久久久久久精品古装| 人妻夜夜爽99麻豆av| 看非洲黑人一级黄片| 91久久精品电影网| 久久99热这里只频精品6学生| 亚洲国产成人一精品久久久| 婷婷色综合大香蕉| 精品卡一卡二卡四卡免费| 国产精品不卡视频一区二区| 观看av在线不卡| 日韩亚洲欧美综合| 在线天堂最新版资源| xxx大片免费视频| 免费在线观看成人毛片| 亚洲欧美精品自产自拍| 精品少妇久久久久久888优播| 人妻系列 视频| 免费大片黄手机在线观看| 久久国产亚洲av麻豆专区| 成人午夜精彩视频在线观看| 伊人亚洲综合成人网| 久久午夜福利片| 秋霞伦理黄片| www.色视频.com| 少妇人妻精品综合一区二区| 大话2 男鬼变身卡| 日韩成人av中文字幕在线观看| 在线观看一区二区三区激情| av在线观看视频网站免费| 日日爽夜夜爽网站| 久久精品国产鲁丝片午夜精品| 日韩av不卡免费在线播放| 免费观看无遮挡的男女| 免费看日本二区| 少妇人妻一区二区三区视频| 日韩亚洲欧美综合| 亚洲av二区三区四区| 国产精品女同一区二区软件| 亚洲人成网站在线观看播放| 搡老乐熟女国产| 夜夜爽夜夜爽视频| 亚洲美女视频黄频| 热re99久久精品国产66热6| 久久久久久久久久久久大奶| 大片免费播放器 马上看| 久久久久久久国产电影| 久久热精品热| 在线观看免费高清a一片| 国产毛片在线视频| 大片电影免费在线观看免费| 狠狠精品人妻久久久久久综合| 亚洲一区二区三区欧美精品| av国产久精品久网站免费入址| 99国产精品免费福利视频| 97在线视频观看| 中文字幕人妻熟人妻熟丝袜美| 亚洲天堂av无毛| 久久久久久久国产电影| 22中文网久久字幕| 午夜免费鲁丝| 日韩成人伦理影院| 一边亲一边摸免费视频| 大又大粗又爽又黄少妇毛片口| 免费不卡的大黄色大毛片视频在线观看| 精品亚洲成国产av| 国产一区二区在线观看日韩| 国产亚洲一区二区精品|