    Multi-stage penetration characteristics of thick ultra-high molecular weight polyethylene laminates

    2023-10-09 04:29:24MingjinCoLiChenRongzhengXuSijiLiuQinFng
    Defence Technology 2023年9期

    Ming-jin Co ,Li Chen ,* ,Rong-zheng Xu ,Si-ji Liu ,Qin Fng ,c

    a Engineering Research Center of Safety and Protection of Explosion & Impact of Ministry of Education,Southeast University,Nanjing,211189,China

    b Institute of Architectural Engineering,Huanghuai University,Zhumadian,463000,China

    c State Key Laboratory of Disaster Prevention & Mitigation of Explosion & Impact,Army Engineering University of PLA,Nanjing,210007,China

    Keywords:UHMWPE laminates Ballistic limit Thickness Mechanism Energy limit

    ABSTRACT To further reveal the failure mechanisms of thick ultra-high molecular weight polyethylene (UHMWPE)laminates,field firing tests were conducted for 10-,20-,and 30-mm thick laminates against 12.7-mm calibre wedge-shaped fragment simulated projectiles at high velocities between 450 and 1200 m/s.The ballistic performance,deformation process,and staged failure characteristics of the laminates with different thicknesses were compared and analysed.The results demonstrate that the ballistic limits of the UHMWPE laminates increase almost linearly with laminate thickness.The 10-mm thick laminate generally experiences two-stage failure characteristics,whereas three-staged failure occurs in the 20-and 30-mm thick laminates and the progressive delamination is evident.The energy limit concept representing the maximum energy absorption efficiency and the idea of reuse of the thick UHMWPE laminates are proposed in this study.The findings of this research will be useful in the design of flexible and effective UHMWPE-based protective equipment.

    1.Introduction

    It was not until World War II that Fibre-reinforced polymerbased materials became extensively developed and progressed.Many high-performance fibres such as glass fibre(E-glass,S-glass)[1-5],carbon fibre (T1100?) [6],aramid fibre (Kevlar?,Twaron?)[7,8],PPID fibre (M5? [9]),PBO fibre (Zylon?) [10],and ultra-high molecular weight polyethylene (UHMWPE) fibre (Dyneema?,Spectra?) [11-14] have been investigated for their excellent performance.Among these,UHMWPE fibres have the lowest density(0.97 g/cm3)and the highest specific strength and specific modulus[15],playing an irreplaceable role in enhancing the manoeuvrability of protective armour while maintaining a high ballistic performance [16-18].

    The effects of laminate thickness [19],lamina stacking angle[20-23],projectile shape [11],penetration angle [24] on the ballistic performance and mechanism of UHMWPE laminates have been explored by researchers.However,most of the projectile velocities were less than 560 m/s,and the thickness of the laminates were mostly within 10 mm.This led to a lack of discussion on the failure mechanism for thicker laminates under high-speed penetration.Tomasz et al.[25] studied the deformation and failure characteristics of 24-mm thick UHMWPE laminates that were impacted by 20-mm calibre fragment simulated projectiles (FSPs)in the velocity range of 400-1000 m/s.They found that there was evident brittle shear failure of the laminates at early penetration stage,and the depth of shear failure increased with the projectile velocity.Moreover,a delamination transition interface that represented the transition from local shear failure to overall bulging deformation in the thick laminate was observed [25],and similar phenomenon was also recognised by Taylor et al.[26],Greenhalgh et al.[27] and Nguyen et al.[28].Heisserer et al.[29] conducted penetration tests on 12.8-mm and 25.5-mm thick UHMWPE laminates against hard steel spheres with a diameter of 5.58 mm(400-1500 m/s),and found that the energy absorption efficiency of the laminates was related to whether the laminates experienced large deformations.However,due to the small diameter of the projectile,the laminates was dominated by shear failure.Greenhalgh et al.[27] studied the ballistic response of 40-mm thick UHMWPE laminates (two 20-mm thick laminates bonded together).They found that the laminates experienced shear failure on the strike face with a bulging deformation on the back face.For the laminates that were processed under a higher processing pressure,the location of the delamination transition interface was further backwards.Nguyen et al.[28] experimentally investigated the ballistic performance and obtained the ballistic limits of UHMWPE laminates with different thicknesses,they demonstrated that the location of the delamination transition interface in the thickness direction was also influenced by the projectile velocity and laminate thickness.However,the real penetration cross sections and failure characteristics of the laminate were not given and discussed in-depth,and the influence of projectile velocity on penetration mechanisms is worth further study and discussion.According to Langston et al.[30],the staged failure mechanism of the laminates is closely related to the form of the analytical model for calculating the penetration resistance.Although many numerical methods [31-34] have been developed to study the ballistic response of UHMWPE laminates,they are mainly used to predict the overall performance of the laminates,and there are still deficiencies in reproducing the opening and staged penetration failure characteristics of UHMWPE laminates [16].Therefore,it is necessary to further experimentally study and recognize the ballistic response and the detailed multi-stage failure mechanisms of the thick UHMWPE laminates.

    In this paper,the anti-penetration performance,deformation process,and opening failure characteristic of 10-,20-,and 30-mm thick UHMWPE laminates under the penetration of 12.7-mm calibre FSPs were investigated.It is believed that this study would be helpful in fully tapping and utilizing the ballistic potential of UHMWPE laminates.

    2.Experimental program

    2.1.Specimen

    The UHMWPE laminates used in this study were produced by the North Jiarui Defense Technology Co.,Ltd.(China),the mechanical property and material composition of the laminates can be referred to Refs.[16,35].The in-plane size of the laminate is 400 × 500 mm2.According to GB/T 32,497-2016 [36],when the distance between impact points is no less than eight times the projectile diameter,and the distance between the impact point and the laminate edge is greater than or equal to 75 mm,the influence of the boundary conditions and the mutual interference of the impacts can be ignored.In addition,for fibre-reinforced composites,to eliminate the influence of fibre pre-damage,the bullets must impact on different fibre bundles each time.Therefore,three points (①-③) are chosen as the impact targets (Fig.1).The four corners of the target laminates are punched by holes (diameter:22 mm) and fixed with bolts (diameter: 20 mm) and washers(external diameter: 40 mm),as shown in Fig.2.

    Fig.1.Positions of the impact points of the laminate.

    Fig.2.Fixed measures of the laminate.

    Fig.3.12.7-mm calibre FSP.

    The projectiles used in this study are 12.7-mm calibre FSPs that made of 40CrNiMoA steel(Rockwell hardness of 30)with a mass of 13.4 g.The appearance of the wedged-shaped FSP is a reference to GB/T 32,497-2016[36],as shown in Fig.3.The FSP is launched by a ballistic gun with sliding chamber,and different initial projectile velocities can be achieved by adjusting the amount of gunpowder.

    2.2.Testing

    Fig.4 gives the ballistic testing layout.After the FSP is launched,the initial and residual velocities are measured by a pair of parallel light screens (trigger accuracy: μs) and a high-speed camera(10,000 FPS),respectively.The deformation process of the laminate are also recorded by the high-speed camera.The high-speed camera is placed on the right-hand side of the laminates and is at the same height as the centre of the laminate(Fig.1).As the highspeed camera is only able to observe the pitch of the FSPs in the vertical direction,to verify the yaw of the FSP in the horizontal direction after penetrating the laminates,a wooden board(Fig.5)is placed behind the laminates to capture the flight paths of the FSP.The results in Fig.5 show that the distances between the centres of the adjacent impact areas on the wooden board (~100 mm) are similar to those(110 mm)designed in Fig.1.In addition,there is no evident offset of the impact points in each area (Fig.5,①-③),which indicates that the FPSs almost fly in straight lines after perforation.Thus,the calculated FSP residual velocities through the high-speed camera are reliable.

    Fig.4.Set-up of the ballistic test.

    Fig.5.Wooden board and the impact points.

    In order to study the anti-penetration mechanism and antipenetration performance of the thick UHMWPE laminates at the same time.The FSP velocities are adjusted to approach the ballistic limits of the laminates through decreasing or increasing the amount of gunpowder,and all the projectile velocities in this study fluctuate within±90 m/s of the ballistic limits.When the difference between the maximum FSP velocity of non-perforation and the minimum FSP velocity of perforation is changing in a very small range(for the 10-,20-,and 30-mm thick laminates were 30,2,and 4 m/s,respectively),it is thought the ballistic limit of the target laminate can be obtained from the average of these two velocities.

    3.Results and analysis

    3.1.Deformation and failure

    3.1.1.Deformation process

    The deformation processes of the UHMWPE laminates recorded the second stage(moments 3-5),with the increase of penetration depth,large area BFD and main delamination interface (MDI,delamination that approximately extends to the edges of the laminate) appears (moment 5,and will be shown in detail in subsection 3.1.3),the laminate shows a global deformation and delamination trend.When the 10-mm thick laminate is impacted by FSP at a velocity of 595.9 m/s,the laminate is perforated and it also experiences a two-stage deformation;however,the deformation degree in the second stage(moments 3-5)is relatively smaller.Owing to the rapid perforation process and the high residual velocity of the FSP (442.9 m/s),the BFD area and BFD depth of the laminate decrease significantly compared to those of nonperforation case and no MDI is observed.The advantage of the UHMWPE fibres-absorbing energy through large tensile deformation-is not fully realised at perforation with high projecby the high-speed camera are presented herein,and they are divided into two cases-critical non-perforation and critical perforation-for each laminate thickness,as shown in Table 1.In general,moment 1 and moment 2 represent the pre and initial contact between the projectile and the laminate,respectively.Moment 3 and moment 4 show the penetration process,where moment 4 shows that the laminate just reaches its largest back face deformation (BFD).Moment 5 gives the final penetration results.

    Table 1 Typical deformation and failure process of the laminates with different thickness.

    When the 10-mm thick laminate is penetrated by FSP at a velocity of 494.5 m/s,its deformation process can be divided into two stages.In the first stage (moments 1-2),the FSP has not entered into the laminate completely,the laminate is dominated by local damage and no evident BFD is observed(as shown in moment 2).In tile residual velocity.

    When the 20-mm thick laminate is impacted by FSP at a velocity of 798.9 m/s,the laminate also experiences a similar two-stage deformation,but it is slightly different from that of the 10-mm thick laminate.In the first stage,brittle shear plugging [28] is more evident due to the fibre and matrix at the impact point are smashed and splashed (as shown in the red box at moment 2).In the second stage(moments 3-5),MDI and large area deformation also appear and the main energy dissipation mode of the laminate is the coupling of delamination and fibre failure.When the 20-mm thick laminate is perforated by FSP at a velocity of 848.0 m/s,breakage occurs and the fibre and matrix are laterally pushed apart at the initial FSP-laminate contact (moment 1),and was also observed by Tomasz[25].Compared to that of non-perforation,the MDI of the perforated 20-mm laminate appears earlier in moment 3.

    When the 30-mm thick laminate is impacted by FSP at a velocity of 1118.5 m/s,the laminate generally shows a three-stage characteristic.In the first stage (moments 1-2),brittle failure occurs at the opening hole,the matrix and fibre debris splash out and the colour of these debris becomes darker than those in the 20-mm thick laminates owing to high-temperature ablation.The second damage stage (moments 3-4) of the 30-mm thick laminate is unique.It can be observed from moment 3 to 4 that several successive MDIs extending to the edges of the laminate appear,which are not observed in the 10-and 20-mm thick laminates.The laminas behind the MDIs are pulled from all sides towards the centre of the impact point,which results in severe expansion of the delamination and bulge deformation.In the third stage(moments 5),the FSP is not capable of perforating the laminate,the remaining energy is dissipated through the extension of in-plane delamination and fibre stretching.When the 30-mm thick laminate is impacted by FSP at a velocity of 1170.7 m/s,the laminate is perforated.However,due to the impact point is located at position ③(Fig.1),which is far from the right-hand edge of the laminate,the progressive penetration and delamination failure are not captured by the high-speed camera.This indirectly reveals that the definition of the global and local damage is related to the size of the laminate.Under perforation,the 30-mm thick laminate also experienced three-stage deformation and failure,which will be described in detail in Subsection 3.1.3.

    3.1.2.Back face deformation depth

    When the FSP velocity exceedsV50of the UHMWPE laminate by approximately tens of metres-per-second,the BFD depth of the laminate reaches its peak value,and the BFD depth in the worst case is selected and analysed conservatively,as shown in Fig.6.The specific FSP velocities for the 10-,20-,and 30-mm thick laminates are 526.0,848.0,and 1153.4 m/s,respectively.In Fig.6,H1represents the maximum BFD depth of the laminate during the FSP-laminate interaction time(IT,time from the warhead contacts the striking face to emerges from the back face),and the values for the 10-,20-,and 30-mm thick laminates are 37.7,31.5,and 50.7 mm,respectively;H2represents the maximum BFD depth of the laminate during the entire deformation process (penetration and free vibration),and the values for the 10-,20-,and 30-mm thick laminates are 37.7,37.9,and 64.1 mm,respectively;H3represents the residual BFD depth of the laminate.

    Fig.6.Time history curves of BFD depths of the laminates.

    The 10-mm thick UHMWPE laminate has the same values ofH1andH2,indicating that the laminate reaches its maximum BFD depth right at the time of perforation.The gradual decline in the slope of the BFD time history curve in Fig.6 represents a decrease in the projectile velocity during the penetration.After reaching the maximum BFD depth,the BFD depth of the 10-mm thick laminate is reduced by 9.2 mm in the thickness direction,and the residualH3is 28.5 mm.

    Due to there is no evident difference in the deformation process of the 20-and 10-mm thick laminates,as illustrated in Table 1,the BFD depth time history of the 20-mm thick laminate is similar to that of the 10-mm thick laminate.However,the value ofH1for the 20-mm thick laminate is slightly smaller than that of the 10-mm thick laminate,which indicates that more critical shearing failure occurred.The 30-mm thick laminate has the largest values ofH1,H2,andH3,and the BFD depth time history curves are significantly different from those of the 10-and 20-mm thick laminates.Firstly,H1for the 30-mm thick laminate is approximately 1.3-1.6 times larger than for the 10-and 20-mm thick laminates.Furthermore,the time interval between theH1andH2of the 30-mm thick laminate is six times larger than that of the 20-mm thick laminate,this implies that the 30-mm thick laminate would experience more severe delamination and in-plane delamination.

    It takes 0.019 ms for the FSP to fly freely at a distance of 10 mm at 526.0 m/s while 0.172 ms to perforate a 10-mm thick laminate.The time consumed during the latter situation is 9.1 times longer than the former.Similarly,the perforation time of the 20-mm thick laminate is 9.1 times the free flight time with an FSP velocity of 848.0 m/s.However,for 30-mm thick laminate,this ratio increases to 13.5 times.This indicates that the 10-and 20-mm thick laminates would have similar deformation process and failure characteristics,whereas the 30-mm thick laminates would be different.

    3.1.3.Failure analysis

    The final penetration failure states of the laminates are shown herein.For the 10-mm thick laminate,it can be observed from Fig.7(a) that the diameter of the holes on the strike face is approximately the same as that of FSP,and there is slight fibre eversion phenomenon at the openings.As shown in Fig.7(b),due to the unidirectional reinforcement and orthogonal stacking sequence of UHMWPE laminas,diamond-shaped bulge areas are formed.However,the adjacent ranges of the bulges are not linked.For the 10-mm thick laminate,the failure characteristics show high similarity under three shots when the velocities of the FSP are approximately 500 m/s.Similar phenomena also appear in the 20-mm thick laminate (FSP:~800 m/s) and 30-mm thick laminates(FSP:~1100 m/s).Succinctly,the failure analysis of one shot can be a reasonable reference for three shots of the 20-or 30-mm thick laminates.

    Fig.7.Failure characteristics of the 10-mm thick laminate: (a) Strike face and impact velocity;(b) Back face and residual velocity.

    As shown in Fig.8(a(2)),evident fibre eversion on the front face is observed for the 20-mm thick laminate.There is no significant difference in the back face deformation and failure between the 10-and 20-mm thick laminates,the diagonal length of the diamondshaped BFD is about 100 mm (the square lattice length on the laminate is 50 mm),as shown in Fig.8(b(1))and Fig.8(b(2)).For the 30-mm thick laminate,with the increase of laminate thickness and FSP velocity,more significant brittle failure and fibre eversion occur on the strike face (Fig.8(a(1))).Owing to the severe delamination failure,the BFD area of the 30-mm thick laminate is larger than and approximately 1.5-2 times those of the 10-and 20-mm thick laminates,as shown in Fig.8(b(3)).During the penetration of the 30-mm thick laminate,the FSP began to undergo slight plastic deformation,which would result in minute degradation of its penetration performance.

    Fig.8.Failure characteristics of the laminates and FSPs: (a) Strike face;(b) Back face;(c) FSP.

    Water jet cutting technique is utilised to obtain the real penetration cross-section of thick UHMWPE laminates.It is experimentally found that the ballistic performance of the UHMWPE laminate varies most significantly around its ballistic limit,thus two cases of critical non-perforation (Fig.9(a)) and critical perforation (Fig.9(b)) are selected for investigation.As shown in Fig.9(a(1)),when the FSP velocity is close to but slightly lower than the ballistic limit of the 10-mm thick laminate,the laminate mainly experiences shear failure.The opening diameter penetrated by the FSP is uniform,and the sidewall of the opening is straight and smooth.The penetrating depth of the 10-mm thick laminate is approximately 7.1 mm when the FSP velocity was 456.8 m/s.When the FSP velocity increased to 526.0 m/s,the 10-mm thick laminate is perforated and shows typical two-stage failure characteristics,as shown in Fig.9(b(1)).Shear plugging failure with uniform opening diameter occurs first,while in the second stage,the laminate experienced large BFD and fibre tension.Moreover,a large MDI that divides the failure from local to global is observed in the laminate,this is caused by the penetration resistance of the back-part laminate that exceeds the interface bonding property between laminas.In comparison to the case when the FSP velocity is slightly lower than the ballistic limit,the delamination and BFD of the laminate at this time are greater and more concentrated,the integrity of each part (stages one and two)of the laminate was well preserved.

    Fig.9.Penetrating failure section of the UHMWPE laminates: (a) Non-perforation;(b) Perforation.

    Fig.9(a(2)) and Fig.9(a(3)) give the cross-sections of the nonperforated 20-and 30-mm thick laminates at FSP velocities of 798.9 and 1118.5 m/s,respectively.And their respective penetration depths are 13.4 and 24.8 mm.It can be observed that when the projectile velocities are slightly lower than the ballistic limits,the 20-and 30-mm thick laminates are dominated by shear failure,and the opening diameters are even across the penetration path.Large number of discrete delamination areas can be observed around the opening holes,similar to those of the 10-mm thick laminates.However,owing to the increase in the laminate thickness and the FSP velocity,one MDI begins to appear in the 20-mm thick laminate and two appear in the 30-mm thick laminate.This indicates that thick UHMWPE laminate is more likely to produce spalling failure in its critical non-perforation state.When the FSP velocities are slightly greater than the ballistic limits,the 20-and 30-mm thick laminates experience typical three-stage penetration and delamination failure,as shown in Fig.9(b(2))and Fig.9(a(3)).Before the first MDI(close to the strike face),the laminates mainly experience shear plugging failure.Between the first and the second MDI,the opening diameters gradually become smaller and the laminas began to bulge,the middle-part laminates experience tension shear coupling failure.Behind the second MDI,the opening diameters continue to decrease and the BFD degree of the laminates become more significant.For the 20-mm thick laminates,regardless of whether the FSP velocities are slightly lower or higher than the ballistic limit,the locations of the MDIs are all near the middle of the thickness direction,and the damage of the first MDI is more evident.For the 30-mm thick laminates,the MDIs are more backward,and the second MDI is the dominant failure interface,the large BFD depth of the 30-mm thick laminate shown in Fig.6 is mainly caused by the lamina deformation behind the second MDI.

    3.2.Ballistic performance

    3.2.1.Ballistic limit

    The experimental FSP velocities and ballistic limits of the UHMWPE laminates are listed in Table 2.The average value method is used to calculateV50of the UHMWPE laminates.Two FSP initial velocitiesViwith the closest value were selected and averaged.One of these two velocities,Vip,is the minimum velocity of perforating the laminate and the other one,Vis,is the maximum velocity of non-perforating the laminate.According to a standard [36],when the difference ofVipandVisis less than 15 m/s,the average of these two values can be regarded as the potentialV50of the laminate.Therefore,the calculated ballistic limits of the 20-and 30-mm thick laminates are 818.2 m/s and 1120.5 m/s,respectively,and the largest coefficients of variation (CoV) of the ballistic limit is 4.3%.TheV50of the 10-mm thick laminate calculated through the average value method is 510.2 m/s,although it does not meet the requirement noted above [36] (the difference ofVipandViswas 31.5 m/s);its accuracy and reliability is verified by the Lambert-Jonas equation (also known as the Recht-Ipson equation[37]).Lambert-Jonas equation has been proven to have strong robustness in predicting the ballistic limit for different materials[38].TheV50calculated through the Lambert-Jonas equation is 515.9 m/s,which is very close to 510.2 m/s and the difference is less than 1.2% and could be ignored.Thus,theV50of the 10-mm thick laminate is taken as 510.2 m/s,and the CoV of the 10-mm thick laminate is approximately 3.2%.

    Table 2 Experimental FSP velocities and ballistic limits of the UHMWPE laminates.

    Average values method

    Lambert-Jonas equation

    where α is a curve fitting parameter,and has a value of 1.23061 in this study.

    whereV1,ipis the minimum FSP velocity of perforation,and should be the first shot of the laminates to ensure conservative.For the 10-20-and 30-mm thick UHMWPE laminates,the values ofV1,ipare 526.0 (approximate value),848.0 and 1170.7 m/s,respectively.

    3.2.2.Energy absorption efficiency

    When the 10-mm thick UHMWPE laminate is non-perforated,the energy dissipated by the laminate increases monotonically with the increase of FSP velocity,as shown in Fig.10(a).However,the maximum energy absorption is not atV50,there is an increase of approximately 5-15% when the FSP velocity is slightly higher thanV50.In this study,the authors propose a concept called energy limit,this concept corresponds to the peak value of the energy absorption and represents the maximum energy absorption capacity of the laminate.The energy limit,to some extent,verified the authenticity of the results that the BFD depth of the UHMWPE laminates reached its peak value at projectile velocities are tens of metres-per-second higher thanV50,as illustrated in Subsection 3.1.2.The 10-mm thick laminate reached its energy limit of approximately 1939.9 J when the FSP velocity was 562.8 m/s,and the energy absorption at this time was 10% higher than that atV50.For the 20-mm thick laminate,the energy limit was not captured in the test owing to the limited number of shots.However,there may be an increase more than 14% in energy absorption at its energy limit in comparison toV50,as shown in Fig.10(b).After perforation,there is a sudden increase in the FSP residual velocity,which is also true for the 30-mm thick laminates,this seems to be unique performance of the thick UHMWPE laminate that the ballistic performance is prone to fluctuate near critical perforation,and needs further studied.For the 30-mm thick laminate,the energy limit is approximately 5% higher thanEbl.The difference between the energy limits andEblof the 30-mm thick laminates becomes smaller than those of the 10-and 20-mm thick laminates,this is because the absolute value ofEblbecomes larger,resulting in a smaller proportion of the difference.

    Fig.10.Residual velocities of the FSPs and the energy absorption of the laminates: (a) 10-mm thick;(b) 20-mm thick;(c) 30 mm-thick;(d) Comparison.

    Before perforation,the maximum energy absorbed by the 10-,20-,and 30-mm thick laminates are 1744.3,4487.5,and 8412.0 J,respectively,and the normalised values are 1.0,2.6,and 4.8,respectively.The normalised energy absorption efficiency per unit thickness of the 10-,20-,and 30-mm thick laminates are 1.0,1.3,and 1.6,respectively.This indicates that the thicker the laminate,the higher its protective efficiency.This is also true for the energy limit.When the FSP initial velocity is lower than that at energy limit,the energy dissipation generally increases with the projectile velocity,and the UHMWPE laminate could give full play to its protective performance.However,when the FSP initial velocity is higher than that at energy limit,the energy dissipation efficiency decreases (probably sharply,as shown in Fig.10(a)) with the increase of the FSP velocity,and the laminate would lose its ballistic advantage.As demonstrated in Fig.10(d),under the penetration of 12.7-mm FSPs,there is approximately a linear positive correlation betweenV50and the laminate thickness,and thus the energy absorption of the UHMWPE laminate approximately has a quadratic relationship with the laminate thickness.

    4.Discussion

    According to the testing observation,thick UHMWPE laminates have large-area delamination trend which would produce predamage of next shot,however,the analysis results show that the existence of pre-damage of the laminates will not lead to significant deviation in the laminate ballistic performance,but within an acceptable range (less than 5%).This means that the testing procedure designed according to standard GB/T 32,497-2016 [36] is reasonable,and the testing results are reliable.For the 10-and 20-mm thick laminates,there are surpluses greater than 10% at energy limits compared toEbl.The energy absorption efficiency of the laminate could be fully exploited in sandwich structures.For the 30 mm thick laminate,there is no significant difference between energy limit andEbl,thus,the ballistic limit could be taken as an indicator in bulletproof design.Due to the sudden increase of FSP residual velocities after just perforating the 20-and 30-mm thick laminates,the ballistic design of thick laminates should be conservative.

    The staged penetration process and severe delamination are unique for thick UHMWPE laminates,and provides the thick laminates with outstanding energy absorption capacity superior to thin UHMWPE laminate.When the FSP velocity is close to the ballistic limit,the BFD depth of the laminates exceeded the value of 25 mm,as specified in standard [39] that is stipulated for body armour.Therefore,to prevent blunt damage,an optimal design should be considered when the UHMWPE laminates are designed to defend the high-speed penetration,such as employing multiple material structures [40,41].Moreover,under the influence of the large deformation and large delamination,the risk of spalling occurs in the back part of the thick laminates,as shown in Fig.11.Therefore,to keep the integrity of the laminate,more attention should be paid to the reliability of the boundary constraints of the laminates.When the 20-and 30-mm thick laminates are impacted by FSPs at velocities higher than the ballistic limits,the integrity of the corresponding part laminates in each penetration stage is well preserved (Fig.9(b(2)) and Fig.9(b(3)).A suggestion can be taken to reuse the penetrated laminates by swapping the front and back faces.The former back part laminates are therefore arranged to experience local shear plugging failure,while the former slightly deformed front faces are arranged as new back faces to experience bulge deformation and delamination.In particular,the idea of reusing is more suitable for the thick laminate because its MDIs are more backward and it has a thicker part of non-delaminated laminate,as illustrated in Fig.9.It can be deduced that the greater the FSP velocity,the more backward the MDIs of the laminate.Therefore,the idea of reusing is more suitable for thick UHMWPE laminate after high-speed penetration.

    Fig.11.Spalling of the thick UHMWPE laminates.

    5.Conclusions

    Multi-stage penetration characteristics of thick UHMWPE laminates against 12.7-mm calibre FSP at velocities of 450-1200 m/s are researched.The main conclusions are as follows:

    (1) The ballistic limits of the 10-,20-,and 30-mm thick laminates are 510.2,818.2,and 1120.5 m/s,respectively,and the ballistic limit increases approximately linearly with the laminate thickness.When the FSP velocity reaches the ballistic limit,the normalised energy absorption efficiencies of the 10-,20-,and 30-mm thick laminates are 1.0,1.3,and 1.6,respectively.

    (2) The 10-mm thick laminate shows two-stage failure characteristics of shear plugging first,bulge deformation and delamination.However,the 20-and 30-mm thick laminates experience more staged penetration process which is influenced by the FSP velocity.Large-area back face deformation and staged delamination are the keys to energy dissipation of thick UHMWPE laminate.

    (3) The maximum BFD depths of the 10-,20-,and 30-mm thick UHMWPE laminates in this research are 37.7,31.5,and 50.7 mm,respectively,which exceed the standard requirements for blunt injury prevention.Thick UHMWPE laminate with single material has limits for defending highspeed steel projectiles,therefore,the multi-material bulletproof plates or sandwich structures are worthy of study in the future.

    Declaration of competing interest

    The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

    Acknowledgements

    The authors acknowledge the financial support from National Natural Science Foundation of China (Grant No.51978166),National Key Research and Development Program of China(Grant No.2019YFC0706105,2021YFC3100703) and the Fundamental Research Funds for the Central Universities (Grant No.2242022R10124s).

    在线观看美女被高潮喷水网站| 美女国产视频在线观看| 久久久久国产网址| 国产精品一区二区在线观看99 | 欧美精品一区二区大全| 国产免费一级a男人的天堂| 免费观看在线日韩| 国内精品美女久久久久久| 国产熟女欧美一区二区| 在线a可以看的网站| 国产精品久久久久久久电影| av.在线天堂| 久久99精品国语久久久| 成人国产麻豆网| 在线免费观看的www视频| 黑人高潮一二区| 嫩草影院精品99| 18禁在线播放成人免费| 欧美一区二区亚洲| 夜夜爽天天搞| 日韩av在线大香蕉| 国产精品嫩草影院av在线观看| 非洲黑人性xxxx精品又粗又长| 女人被狂操c到高潮| 日本三级黄在线观看| 国产探花在线观看一区二区| 亚洲成av人片在线播放无| 老熟妇乱子伦视频在线观看| 日本成人三级电影网站| 91午夜精品亚洲一区二区三区| 97人妻精品一区二区三区麻豆| 日韩中字成人| 国产亚洲91精品色在线| 国产精品一区www在线观看| 波野结衣二区三区在线| 午夜精品在线福利| 黄片无遮挡物在线观看| 99久久精品一区二区三区| 少妇人妻一区二区三区视频| 伦精品一区二区三区| 日日干狠狠操夜夜爽| 精品久久久久久久久亚洲| av天堂中文字幕网| 欧美另类亚洲清纯唯美| 少妇猛男粗大的猛烈进出视频 | 岛国毛片在线播放| 一级毛片久久久久久久久女| 一区福利在线观看| 欧美+亚洲+日韩+国产| 十八禁国产超污无遮挡网站| 1024手机看黄色片| av在线播放精品| 日本爱情动作片www.在线观看| 午夜免费激情av| 久久久午夜欧美精品| 亚洲国产精品合色在线| 久久久国产成人精品二区| 精品一区二区免费观看| 人妻制服诱惑在线中文字幕| 国产亚洲精品av在线| 日韩一区二区视频免费看| 国产探花在线观看一区二区| 国产av一区在线观看免费| 91在线精品国自产拍蜜月| 久久精品国产自在天天线| 99视频精品全部免费 在线| 亚洲av不卡在线观看| 日韩高清综合在线| 午夜a级毛片| 国产av麻豆久久久久久久| 久久久国产成人免费| 国产真实乱freesex| 女人十人毛片免费观看3o分钟| 亚洲av.av天堂| 只有这里有精品99| 99久久九九国产精品国产免费| 久久久色成人| 丝袜美腿在线中文| 超碰av人人做人人爽久久| 国产黄色小视频在线观看| а√天堂www在线а√下载| 精华霜和精华液先用哪个| av天堂中文字幕网| 中文资源天堂在线| 欧美最黄视频在线播放免费| 亚洲aⅴ乱码一区二区在线播放| 免费av毛片视频| 天堂中文最新版在线下载 | 一进一出抽搐gif免费好疼| 亚洲人成网站在线观看播放| 中文字幕av在线有码专区| 国产精品乱码一区二三区的特点| 欧美人与善性xxx| 联通29元200g的流量卡| 日本撒尿小便嘘嘘汇集6| 日韩高清综合在线| 精品免费久久久久久久清纯| 国产黄色小视频在线观看| 一本久久中文字幕| 久久久精品欧美日韩精品| 久久精品久久久久久噜噜老黄 | 午夜福利成人在线免费观看| 卡戴珊不雅视频在线播放| 国国产精品蜜臀av免费| 22中文网久久字幕| 国产高清不卡午夜福利| 国产午夜精品论理片| 成年免费大片在线观看| 久久久久九九精品影院| 亚洲av.av天堂| 国产一区二区三区av在线 | 欧美zozozo另类| 亚洲aⅴ乱码一区二区在线播放| 精品免费久久久久久久清纯| 在线免费观看的www视频| 久久精品国产亚洲av香蕉五月| 久久精品久久久久久噜噜老黄 | 少妇人妻一区二区三区视频| 蜜臀久久99精品久久宅男| 国产老妇女一区| 精品少妇黑人巨大在线播放 | 人人妻人人看人人澡| 两性午夜刺激爽爽歪歪视频在线观看| 丝袜喷水一区| a级毛色黄片| 色播亚洲综合网| 日韩成人av中文字幕在线观看| 看非洲黑人一级黄片| 小说图片视频综合网站| 婷婷亚洲欧美| 夫妻性生交免费视频一级片| 成人欧美大片| 午夜免费男女啪啪视频观看| 联通29元200g的流量卡| 亚洲av成人精品一区久久| 日韩一区二区三区影片| 99久国产av精品国产电影| 全区人妻精品视频| 欧美另类亚洲清纯唯美| 老司机影院成人| av又黄又爽大尺度在线免费看 | 十八禁国产超污无遮挡网站| 欧美高清性xxxxhd video| 亚洲一区高清亚洲精品| 亚洲成a人片在线一区二区| 一本一本综合久久| 夜夜爽天天搞| 最近中文字幕高清免费大全6| 欧美激情在线99| 欧美激情在线99| 激情 狠狠 欧美| 亚洲国产欧美人成| 男女下面进入的视频免费午夜| 91aial.com中文字幕在线观看| 久久精品国产自在天天线| 3wmmmm亚洲av在线观看| 午夜a级毛片| 国产成年人精品一区二区| 99久久中文字幕三级久久日本| 美女黄网站色视频| 少妇的逼好多水| 亚洲最大成人av| а√天堂www在线а√下载| 国产一区二区在线av高清观看| 18禁在线播放成人免费| АⅤ资源中文在线天堂| 日韩欧美一区二区三区在线观看| 亚洲国产欧洲综合997久久,| 国国产精品蜜臀av免费| 深爱激情五月婷婷| 久久精品影院6| 国产av不卡久久| 少妇被粗大猛烈的视频| 成人三级黄色视频| 亚洲成人中文字幕在线播放| 成人国产麻豆网| av在线观看视频网站免费| 少妇熟女aⅴ在线视频| 中文字幕av在线有码专区| 国产av麻豆久久久久久久| 久久久久久久久久成人| 国产精品.久久久| 亚洲第一区二区三区不卡| 日韩欧美在线乱码| 国产亚洲av片在线观看秒播厂 | 国产视频内射| 美女高潮的动态| 色视频www国产| 亚洲久久久久久中文字幕| 又爽又黄无遮挡网站| 99热全是精品| 韩国av在线不卡| 国产精品蜜桃在线观看 | 久久久久久久亚洲中文字幕| 可以在线观看毛片的网站| 国产午夜精品一二区理论片| 久久久欧美国产精品| 久久久久久久久中文| 国产色婷婷99| 精品人妻一区二区三区麻豆| 日本一本二区三区精品| 日本一本二区三区精品| 日韩视频在线欧美| 久久久久久久久中文| 搞女人的毛片| 国语自产精品视频在线第100页| av天堂中文字幕网| 日产精品乱码卡一卡2卡三| 亚洲av成人av| 我要看日韩黄色一级片| 校园人妻丝袜中文字幕| 18禁在线无遮挡免费观看视频| 午夜老司机福利剧场| 最近中文字幕高清免费大全6| 亚洲国产精品成人综合色| 麻豆成人午夜福利视频| 亚洲人成网站在线播| 欧美一级a爱片免费观看看| 亚洲欧美日韩东京热| 白带黄色成豆腐渣| 夫妻性生交免费视频一级片| 国产亚洲精品久久久久久毛片| 亚洲精品乱码久久久久久按摩| 亚洲欧美日韩无卡精品| 久久婷婷人人爽人人干人人爱| 最新中文字幕久久久久| 亚洲欧美成人综合另类久久久 | 亚洲精品日韩在线中文字幕 | 成人av在线播放网站| 亚洲欧美精品综合久久99| 亚洲在线观看片| 国产午夜精品论理片| 乱码一卡2卡4卡精品| 少妇高潮的动态图| 91狼人影院| 国产伦理片在线播放av一区 | 黄色一级大片看看| 不卡一级毛片| 国产精品无大码| 久久99热这里只有精品18| av又黄又爽大尺度在线免费看 | 人体艺术视频欧美日本| 日韩人妻高清精品专区| 亚洲欧美成人综合另类久久久 | 色吧在线观看| 日韩强制内射视频| 欧美成人一区二区免费高清观看| 老司机福利观看| 国产综合懂色| 午夜视频国产福利| 欧美日韩国产亚洲二区| 亚洲欧美日韩东京热| ponron亚洲| 免费av毛片视频| 亚洲欧洲日产国产| 精品久久久久久久久av| 国产精品久久视频播放| 男插女下体视频免费在线播放| 99国产精品一区二区蜜桃av| 久久人人爽人人片av| 国产亚洲av片在线观看秒播厂 | 熟女电影av网| 身体一侧抽搐| 中文字幕av成人在线电影| 久久这里只有精品中国| 亚洲国产欧美人成| 欧美日韩在线观看h| 亚洲一级一片aⅴ在线观看| 久久久久久大精品| 99久久精品国产国产毛片| 麻豆av噜噜一区二区三区| 久久精品久久久久久久性| 极品教师在线视频| 亚洲在线观看片| 免费一级毛片在线播放高清视频| 99精品在免费线老司机午夜| 欧美日韩国产亚洲二区| 国语自产精品视频在线第100页| 嘟嘟电影网在线观看| 国产淫片久久久久久久久| 中文在线观看免费www的网站| 国产精品野战在线观看| 国产午夜福利久久久久久| 在线天堂最新版资源| 国产精品无大码| 九九久久精品国产亚洲av麻豆| 国产精品免费一区二区三区在线| 99九九线精品视频在线观看视频| 性色avwww在线观看| 女人被狂操c到高潮| 大又大粗又爽又黄少妇毛片口| 日本成人三级电影网站| 亚洲自拍偷在线| 亚洲av免费在线观看| 乱人视频在线观看| 久久九九热精品免费| 麻豆精品久久久久久蜜桃| 国产精品麻豆人妻色哟哟久久 | 亚洲精品久久久久久婷婷小说 | 看片在线看免费视频| 日韩国内少妇激情av| 国产女主播在线喷水免费视频网站 | 99国产精品一区二区蜜桃av| 亚洲欧美日韩高清专用| 十八禁国产超污无遮挡网站| 亚洲电影在线观看av| 91aial.com中文字幕在线观看| 九九热线精品视视频播放| 性色avwww在线观看| 尤物成人国产欧美一区二区三区| 黄色配什么色好看| 男女做爰动态图高潮gif福利片| 午夜福利在线观看吧| 精品久久久久久成人av| 一级黄色大片毛片| 高清午夜精品一区二区三区 | 免费搜索国产男女视频| 国产黄色视频一区二区在线观看 | 国产探花在线观看一区二区| 日韩精品青青久久久久久| 日韩成人av中文字幕在线观看| 桃色一区二区三区在线观看| 国产在线精品亚洲第一网站| 成人av在线播放网站| 欧美最黄视频在线播放免费| 久久精品人妻少妇| 久久精品综合一区二区三区| 一进一出抽搐动态| 黄色欧美视频在线观看| 岛国毛片在线播放| 少妇人妻一区二区三区视频| 久久人人爽人人片av| 国产麻豆成人av免费视频| 看黄色毛片网站| av天堂在线播放| 欧美性感艳星| 一级av片app| 中国美白少妇内射xxxbb| 色噜噜av男人的天堂激情| 青春草亚洲视频在线观看| 男人的好看免费观看在线视频| 午夜精品国产一区二区电影 | 男人和女人高潮做爰伦理| 色尼玛亚洲综合影院| 三级经典国产精品| 国产蜜桃级精品一区二区三区| 一区二区三区免费毛片| 99久久成人亚洲精品观看| 三级男女做爰猛烈吃奶摸视频| 亚洲精品成人久久久久久| 少妇裸体淫交视频免费看高清| 女人被狂操c到高潮| 欧美日韩国产亚洲二区| 亚洲成人精品中文字幕电影| 偷拍熟女少妇极品色| 夜夜夜夜夜久久久久| 两性午夜刺激爽爽歪歪视频在线观看| 亚洲成人精品中文字幕电影| 搡老妇女老女人老熟妇| 精品99又大又爽又粗少妇毛片| 亚洲成人av在线免费| 高清日韩中文字幕在线| 欧美色视频一区免费| 国产激情偷乱视频一区二区| 国产三级中文精品| 一夜夜www| 国产乱人偷精品视频| 欧美三级亚洲精品| 中文精品一卡2卡3卡4更新| 午夜激情欧美在线| 老熟妇乱子伦视频在线观看| 日韩欧美一区二区三区在线观看| 性色avwww在线观看| 一级毛片aaaaaa免费看小| 22中文网久久字幕| 欧美性感艳星| 成人二区视频| 国产探花极品一区二区| 国产不卡一卡二| 亚洲四区av| 少妇的逼水好多| 亚洲欧美精品专区久久| 亚洲av一区综合| 亚洲美女搞黄在线观看| 成年女人看的毛片在线观看| 亚洲无线在线观看| 干丝袜人妻中文字幕| 免费看光身美女| 热99在线观看视频| 久久久久网色| 国产精品野战在线观看| 日日啪夜夜撸| 青青草视频在线视频观看| 亚洲av不卡在线观看| 亚洲成人av在线免费| 国产精品一区二区三区四区久久| 一进一出抽搐动态| 国产毛片a区久久久久| 美女黄网站色视频| 秋霞在线观看毛片| 久久久久国产网址| 免费不卡的大黄色大毛片视频在线观看 | 国产成人aa在线观看| 国产精品乱码一区二三区的特点| 亚洲美女视频黄频| 老司机影院成人| 久久久久免费精品人妻一区二区| 婷婷色综合大香蕉| 性插视频无遮挡在线免费观看| 最近最新中文字幕大全电影3| 亚洲精品乱码久久久久久按摩| 舔av片在线| 老司机福利观看| 熟女电影av网| 亚洲av一区综合| 亚洲第一电影网av| 中文字幕av成人在线电影| 日本av手机在线免费观看| 午夜精品一区二区三区免费看| 波多野结衣高清无吗| 亚洲av第一区精品v没综合| 99久久成人亚洲精品观看| 此物有八面人人有两片| 免费搜索国产男女视频| a级一级毛片免费在线观看| 搡女人真爽免费视频火全软件| videossex国产| 亚洲在线观看片| 国产乱人视频| 亚洲四区av| 久久久久久久久久久免费av| 欧美性感艳星| 日韩一区二区视频免费看| 99热网站在线观看| 亚洲人与动物交配视频| 少妇的逼水好多| 国产精品福利在线免费观看| 国产亚洲av嫩草精品影院| 久久久久久久久中文| 菩萨蛮人人尽说江南好唐韦庄 | 三级国产精品欧美在线观看| 中国国产av一级| 亚洲图色成人| 国产爱豆传媒在线观看| 嫩草影院新地址| 日本一本二区三区精品| 国产av在哪里看| 亚洲五月天丁香| 美女被艹到高潮喷水动态| 婷婷色综合大香蕉| 国产精华一区二区三区| 成人午夜高清在线视频| 男人舔奶头视频| 99riav亚洲国产免费| 人人妻人人看人人澡| 日韩欧美三级三区| 一级av片app| 精品熟女少妇av免费看| 国产高清有码在线观看视频| 成人综合一区亚洲| 26uuu在线亚洲综合色| 狂野欧美白嫩少妇大欣赏| 在线a可以看的网站| or卡值多少钱| 亚洲av成人精品一区久久| 深夜a级毛片| 国产片特级美女逼逼视频| 美女脱内裤让男人舔精品视频 | 国产精品爽爽va在线观看网站| 亚洲图色成人| 波多野结衣高清无吗| 国产精品久久久久久av不卡| 国产精品野战在线观看| avwww免费| 日韩一区二区三区影片| 国产精品久久久久久久电影| 国产精品爽爽va在线观看网站| 亚洲国产精品国产精品| 神马国产精品三级电影在线观看| 国模一区二区三区四区视频| 亚洲欧美成人精品一区二区| 99久久精品热视频| 成人鲁丝片一二三区免费| 欧美一区二区精品小视频在线| 日韩av在线大香蕉| av在线亚洲专区| 淫秽高清视频在线观看| 又爽又黄a免费视频| 91av网一区二区| 久久精品夜色国产| 边亲边吃奶的免费视频| 亚洲高清免费不卡视频| 一个人看视频在线观看www免费| a级毛片免费高清观看在线播放| 丝袜喷水一区| 日韩欧美一区二区三区在线观看| 成人二区视频| 又粗又爽又猛毛片免费看| 毛片女人毛片| 久久久久久久久久久免费av| 激情 狠狠 欧美| 日韩视频在线欧美| 久久99热这里只有精品18| 久久99热6这里只有精品| 亚洲第一区二区三区不卡| 亚洲婷婷狠狠爱综合网| 一个人看视频在线观看www免费| 精品久久国产蜜桃| 久久久久久久久久久丰满| 国产精品综合久久久久久久免费| 一边摸一边抽搐一进一小说| 色5月婷婷丁香| 一边亲一边摸免费视频| 蜜桃久久精品国产亚洲av| 久久久午夜欧美精品| 国产亚洲精品久久久com| 婷婷亚洲欧美| 听说在线观看完整版免费高清| 亚洲人成网站高清观看| 最新中文字幕久久久久| 久久久久性生活片| 久久精品91蜜桃| 日韩一区二区视频免费看| 欧美bdsm另类| 人妻久久中文字幕网| 看非洲黑人一级黄片| 精品日产1卡2卡| 此物有八面人人有两片| 午夜精品在线福利| 国产亚洲精品久久久久久毛片| а√天堂www在线а√下载| 小蜜桃在线观看免费完整版高清| 变态另类丝袜制服| 啦啦啦观看免费观看视频高清| 久久久久久伊人网av| 午夜激情欧美在线| 村上凉子中文字幕在线| 成年免费大片在线观看| 中文欧美无线码| 日本黄色片子视频| 此物有八面人人有两片| 人妻少妇偷人精品九色| 国产精品久久久久久久电影| 岛国在线免费视频观看| 欧美日本视频| av又黄又爽大尺度在线免费看 | 久久中文看片网| 国产精品久久电影中文字幕| 欧美日韩在线观看h| 可以在线观看的亚洲视频| 人妻夜夜爽99麻豆av| 亚洲欧美日韩高清专用| 国产极品精品免费视频能看的| 男人和女人高潮做爰伦理| 亚洲欧美精品自产自拍| 亚洲最大成人手机在线| 99视频精品全部免费 在线| 天美传媒精品一区二区| 特级一级黄色大片| 免费观看人在逋| 欧美日本视频| a级毛片a级免费在线| 黄色欧美视频在线观看| 国产成年人精品一区二区| 国产日韩欧美在线精品| 哪里可以看免费的av片| 欧美一级a爱片免费观看看| 亚州av有码| 亚洲在线观看片| 亚洲熟妇中文字幕五十中出| 又黄又爽又刺激的免费视频.| 我的女老师完整版在线观看| 国产精品永久免费网站| 搡女人真爽免费视频火全软件| 人妻久久中文字幕网| 18禁黄网站禁片免费观看直播| 亚洲一区高清亚洲精品| 免费看a级黄色片| 日本撒尿小便嘘嘘汇集6| 午夜福利在线在线| 少妇熟女欧美另类| 日本五十路高清| 午夜激情福利司机影院| 日韩av不卡免费在线播放| 国产精品美女特级片免费视频播放器| 12—13女人毛片做爰片一| 亚洲欧美日韩高清专用| 波野结衣二区三区在线| 卡戴珊不雅视频在线播放| 国产精品.久久久| 国产成人a∨麻豆精品| 九草在线视频观看| 日本爱情动作片www.在线观看| 色5月婷婷丁香| 少妇裸体淫交视频免费看高清| 国产免费男女视频| 亚洲av第一区精品v没综合| 黄色一级大片看看| 国产精品久久久久久av不卡| 一级黄色大片毛片| 久久久久九九精品影院| 九九在线视频观看精品| 最后的刺客免费高清国语| 在线观看免费视频日本深夜| 午夜老司机福利剧场| 欧美区成人在线视频| 99久久精品国产国产毛片| 身体一侧抽搐| 能在线免费观看的黄片| 男人舔奶头视频| 久久精品久久久久久久性| 亚洲欧美日韩东京热| а√天堂www在线а√下载| 99久久九九国产精品国产免费| 亚洲高清免费不卡视频|