    Experimental and numerical studies of titanium foil/steel explosively welded clad plate

    2023-07-31 13:30:56ZhixiongBiXuejioLiKeYngRongKiQunWngMengenXuTingzhoZhngXindeDiJingyeQinYongWu
    Defence Technology 2023年7期

    Zhi-xiong Bi ,Xue-jio Li ,Ke Yng ,Rong Ki ,Qun Wng ,Meng-en Xu ,Ting-zho Zhng ,Xin-de Di ,Jing-ye Qin ,Yong Wu

    a School of Civil Engineering, Anhui University of Science and Technology, Huainan, Anhui, 232001, PR China

    b School of Chemical Engineering, Anhui University of Science and Technology, Huainan, Anhui, 232001, PR China

    cSchool of Mining Engineering, Anhui University of Science and Technology, Huainan, Anhui, 232001, PR China

    Keywords:Explosive welding Pressure transfer layer Titanium foil Simulation Bonding property

    ABSTRACT Ti/Fe clad plate had attracted extensive attention because of its important application.In order to reduce the titanium layer thickness,the explosive welding of TA1 titanium foil to Q235 steel plate was carried out.The interfacial bonding performance was analyzed by micromorphology analysis and mechanical property test,and the formation process of interfacial wave and molten block in the vortex was simulated by smoothed particle hydrodynamics (SPH) method.The results showed that salt as pressure transfer layer used in explosive welding could play a good buffer effect on the collision between flyer and base layers.Regular waveforms were formed on the bonding interface,and the titanium foil/steel clad plate exhibited good welding quality and bonding property.The crest of the observed interfacial wave moved 200 μm from the beginning to the final formation,and it was important of jet on the formation of interfacial waveform.The interface was mainly bonded in the form of molten layer,and the grains near the interface were streamlined.Molten block containing intermetallic compounds and metal oxides appeared in the vortex of wave crest.

    1.Introduction

    Titanium could rapidly form a stable oxidizing protective film in air or solution[1-4].Ti/Fe clad plate has both corrosion resistances of titanium and toughness of steel,which has great utilization potentiality in chemical equipment,power generation assembly and ocean engineering [5-7].Explosive welding is an important processing method for Ti/Fe clad plate,which converts chemical energy released by explosive detonation into kinetic energy of flyer layer to achieve metallurgical bonding between the two metallic plates [8-11].Flyer layer for explosive welding needs to collide with base layer at high speed,thus the thickness of flyer layer is generally more than 2 mm to withstand explosion load [12-15].However,titanium layer with a thickness of 400 nm could play a corrosion resistance effect [1,2,16].

    Due to the excellent bonding ability and corrosion resistance,it has drawn increasing interest in the explosive welding of titanium to steel.In Ning et al.'s work,Zr/Ti/Fe clad plate was fabricated by explosive welding,and their microstructure and mechanical properties were studied.The corrosion resistance of zirconium and titanium in the trilaminar clad plate was complementary[14].Song et al.[7] explored the microstructure of explosive cladding joints formed among parallel titanium and steel plates and found the bonding interface formed pronounced hierarchical microstructures.Somasundaram et al.[15] investigated the interfacial structure and corrosion resistance of TA1/304L clad plate by changing mass ratio and preset angle.The microstructural study revealed the transformation from straight to wavy interface while increasing loading ratios,and the clad plate has superior performance in corrosion environment because of the formation of titanium oxide layer.In Chu et al.’s study[12],low carbon steel and pure titanium were welded by explosive welding,and intermetallic compounds of Fe2Ti and FeTi were found at the bonding interface.Zhou et al.[6]investigated the tensile shear failure mechanism and mechanical properties of TA2/Q235 clad plate.The tensile shear failure mainly occurred along the interfacial wave direction and was caused by the defects of cavities,cracks and brittle intermetallic compounds.

    The cladding thickness of clad plate might only need a few hundred microns to meet the performance requirements.Many attempts had been made to realize explosive welding of metallic foil,and the bonding properties and interfacial formation mechanism of clad plates were investigated by numerical simulation,mechanical property testing and microstructure analysis.In Yang et al.’s study[11],aluminum plate as a protective layer was placed between explosive and tantalum foil,and the tantalum foil was successfully welded to steel plate by improving traditional explosive welding technology.The microstructures of welded joints were analyzed by scanning electron microscope (SEM) and energy disperse spectroscopy (EDS),and the corrosion resistance of Ta/Fe clad plate was investigated by corrosion test.Inao et al.[17] reported that the explosive welding of aluminum foil to magnesium alloy plate was successfully realized by adding gel material as pressure transfer layer to the surface of aluminum foil,and the attenuation effect of gel material on collision energy was studied.Yang et al.[18] explored a double-layer structure consisted of a cardboard and a thin aluminum plate as a buffer layer to reduce the surface ablation and stress wave damage of copper foil/steel explosive welding.The interface evolutions,nanomechanical properties and relevant governing mechanisms of copper foil/steel welding system were investigated by SPH simulation method and advanced characterization.In Liu’s work[19],the metallic glass foil was attached on a driver plate,and an aluminum plate was coated by a Fe-based metallic glass foil.The explosive welding process was simulated by a self-developed code and the bonding mechanism was studied by numerical analysis.The buffer materials used above were inevitably damaged under the explosion load and could not be reused.

    In this work,the explosive welding of titanium foil to steel plate was studied by using low detonation velocity emulsion explosive as welding charge and salt as pressure transfer layer.Microstructure evolution of the welding interface was characterized by optical microscope(OM),scanning electron microscope(SEM)and energy disperse spectroscopy (EDS).The mechanical property was measured by tensile and bending tests.The explosive welding process was simulated by smoothed particle hydrodynamics(SPH)method.

    2.Materials and models

    2.1.Experimental procedure

    A TA1 titanium plate with a dimension of 200 μm × 100 mm × 200 mm was bonded to a Q235 steel with a dimension of 15 × 100 × 200 mm3.The chemical composition of participant metals is given in Table 1.

    Table 1 Chemical composition of TA1 titanium and Q235 steel.(mass fraction%).

    Based on emulsion matrix(Table 2),hollow glass microspheres were used as sensitizer and diluent to prepare low detonation velocity emulsion explosive with 20% microsphere content,whose density was 685 kg/m3and detonation velocity was 3148 m/s.Aluminum honeycomb plate was used as explosive frame,which had good compressive resistance and could ensure uniform charge thickness.Honeycomb structure explosive with a thickness of12 mm was prepared by filling honeycomb pores with the emulsion explosive,specific parameters of aluminum honeycomb panel could be found in previous work[20].A 5 mm thick salt layer was placed on the surface of flyer plate as pressure transfer layer.Salt crystal was liquefied under the high temperature of 1079 K,which could protect titanium foil from high temperature burn and reduce impact load damage [21,22].

    Table 2 Emulsion matrix component.(mass fraction%).

    A parallel structure was employed to the explosive welding assembly,as shown in Fig.1.The stand-off distance between base and flyer layers was 4 mm.The inner surfaces of the titanium foil and steel plate were polished,and the welding assembly was placed on the foundation of spherical tank.The initiating end was located on the left part of the charge.

    Fig.1.Assembly drawing of explosive welding of TA1 titanium to Q235 steel.

    After explosive welding,the specimens for microscopic morphology analysis were cut parallel to the direction of detonation by wire cutting machine.The position of the specimen was 100 mm away from the initiation end,which can avoid unstable detonation effect of the explosive in the initiation end.The general morphology was checked via OM(Carl Zeiss Axio Imager A1m)and SEM (Phenom ProX).The mechanical properties were tested by universal testing machine (MTS 810).

    2.2.Explosive welding simulation

    2.2.1.Collision velocity

    A 2D planar model was developed in ANSYS/AUTODYN code for the explosive welding of TA1 titanium foil to Q235 steel plate.The SPH processor exhibited advantages in accurately simulating the deformation behavior of materials [23,24].The parameters of emulsion explosive and salt in the simulation were consistent with those in the experiment.To obtain the collision velocity between flyer and base plates,2D simulation based on ANSYS/AUTODYN code was carried out.The flyer material was TA1 titanium with a thickness of 200 μm,and the base material was Q235 steel with a thickness of 15 mm.The stand-off distance between base and flyer layers was 4 mm.A gauges point was set on the inner surface of flyer layer every 3 mm,as shown in Fig.2.The particle size was 0.1 × 0.1 mm2,and there were 96,600 particles in the model.

    Fig.2.Assembly drawing of explosive welding.

    Jones-Wilkins-Lee (JWL) equation of state (EOS) was used for the explosive,and its calculation formula was as follows [25]:

    wherePis the detonation product pressure,AJ,BJ,R1,R2and ω are the material coefficients,E0is the initial specific internal energy,and V0is the relative specific volume of detonation gas products.The state parameters of the emulsion explosive are listed in Table 3.

    Table 3 Jones-Wilkins-Lee equation of state parameters of explosive.

    Pressure transfer layer was modelled using Compaction equation of state and Mo Granular material model,which had better simulation effect for granular material.Compaction equation of state is often used to describe granular materials,and its calculation formula was as follows [26]:

    wherePis the pressure,a,c,d,and λ are constant parameters that will be determined based on various curve fitting techniques.ρ0is the initial density of the material,ρHis the current density of the material.

    The pressure transfer layer was formed by salt particles,and the density of salt particles with various sizes was different.In order to reduce the differences to achieve better simulation effect.Different initial parameters were set for Compaction equation of state and Mo Granular material model.In the work,four kinds of particles were set to form the pressure transfer layer,the initial densities salt of salt particles with the same size were shown in Table 4.

    Table 4 Compaction equation of state parameters of pressure transfer layer.

    The Mo Granular material model can be described as [27].where σY,σP,σρand F denote the total yield stress,the pressure yield stress,the density yield stress and the pressure of granular respectively.Accordingly,pressure yield stress and the density yield stress of pressure transfer layers composed of the four kinds of particles were shown in Table 5.

    Table 5 Mo Granular material model parameters of pressure transfer layer.

    where ρ is the material density,Γ0is the Grüneisen coefficient,c0is the volumetric sound velocity,sis the material constant,eis the inner energy,c0is the bulk sound velocity.The specific parameters of the Mie-Gruneisen equation of state of TA1 titanium and Q235 steel are shown in Table 6.

    Table 6 Mie-Gruneisen equation of state parameters of TA1 titanium and Q235 steel.

    Johnson-Cook material model was used as the constitutive model for Q235 steel,which could be expressed as [30,31].

    where εPis the effective plastic strain;is the effective plastic strain rate;A,B,C,m and n are the correlation constants of materials,T2is the particle temperature,T* is the dimensionless temperature,Tris the reference temperature,Tmis the melting point.The specific parameters of Johnson-Cook material model of Q235 steel were shown in Table 7.

    Table 7 Johnson-Cook material model parameters for Q235 steel.

    Steinberg-Guinan material model was used as the constitutive model for TA1 titanium,which described the expressions of shear modulus and flow stress before material melting as [32-34].

    whereYis the flow stress,μ is the shear modulus,is the equivalent plastic strain,V1is the relative volume,Y0,β1,n,μ0,b,h and T1are the given medium constants.The specific parameters of the Steinberg-Guinan material model for TA1 titanium were shown in Table 8.

    Table 8 Steinberg-Guinan material model parameters for TA1 titanium.

    2.2.2.Collision simulation

    In order to obtain TA1/Q235 explosive welding parameters and study the formation mechanism of wavy interface,the collision velocities of 11 gauges points were obtained by explosive welding simulation,and the collision angles of the corresponding collision velocities were calculated.The formula for calculating the collision angle with parallel installation structure could be expressed as[35,36].

    wherevpis the collision velocity,vcis the collision point velocity,β is the collision angle,and vdis the detonation velocity of explosive.

    The critical collision velocity between dissimilar metal plates was given by the following formula [37]:

    When the girl had finished she went back to find the cows, but they had gone, and though she hunted everywhere she never found them; and she had to return home and confess to her master, who scolded her bitterly, and afterwards beat her

    wherevp,minis the critical velocity,vp1andvp2are the minimum collision velocity between flyer layers and between base layers,respectively,p1andp2are the collision pressure between flyer layers and between base layers,respectively,CV1andCV2are the volume sound velocities of flyer and base layers,respectively,ρ1and ρ2are the density of flyer and base layers,respectively,and σb1and σb2are the tensile strengths of flyer and base layers,respectively.

    According to the fluid mechanics theory,when the collision point velocity exceeded its lower limit,the interfacial metal transformed from laminar flow to turbulent flow,resulting in a wavy bonding.For the critical collision point velocity,the formula was as follows [38]:

    wherevc,minis the critical collision point velocity,Reis the Reynolds number,andH1andH2are the Vickers hardness of flyer and base plates,respectively.

    Walsh et al.[39] proposed that the ultimate collision velocity between dissimilar metal plates could be expressed as

    wherevp,maxis the ultimate collision velocity,CP1andCP2are the specific heat capacities of flyer and base layers,respectively,α1and α2are the thermal diffusivity of flyer and base layers,respectively,C1and C2are the sonic speed of flyer and base layers,respectively,δ1and δ2are the thickness of flyer and base layers,respectively,Tmpminis the lower melting point of flyer and base layers,tminis the shortest time for the sparse waves to reflect to the bonding interface,and N is the coefficient related to the sonic speed of material.

    In explosive welding,a large enough collision angle was required for the interfacial metal to produce jet.Therefore,the formula of ultimate collision point velocity was proposed by collision angle [40].

    wherevc,maxis the ultimate collision point velocity.

    An oblique collision assembly was used to focus on the collision process of Ti/Fe explosive welding in the simulation model,as shown in Fig.3.In order to save calculation time,the size of TA1 titanium as flyer layer was 200 μm×10 mm,and the size of Q235 steel as base layer was 0.5×10 mm2.The equation of state,material model and numerical simulation method remained unchanged.The particle size was reduced to 4 × 4 μm2,and there were 437,500 particles in the model,which could be enough to get accurate simulation results.The collision angles were calculated according to the collision velocities of the 11 gauges points,as shown in Table 9.

    Fig.3.Schematic diagram of oblique collision model.

    Table 9 Collision velocities and collision angles in the model.

    3.Results and discussion

    3.1.Simulation results of TA1/Q235 explosive welding

    The upper limit and lower limit parameters of TA1/Q235 weldability window were calculated according to Eq.(13) to Eq.(20),as shown in Table 10.

    Table 10 Weldability window parameters for TA1/Q235 explosive welding.

    The critical collision velocity and limit collision velocity of the welding mode were 423 m/s and 2027 m/s,respectively,which was marked by dotted lines in Fig.4.

    The collision velocities of the welding models were all higher than the critical collision velocities,which indicated that the parameters used for explosive welding of titanium foil to steel plate were reasonable [41].The starting and ending points of the explosive were affected by sparse wave,where the collision velocity was small [10].However,the detonation velocity increased and tended to be stable as the detonation transmission distance increased.

    According to the parameters in Table 10,the weldability window was obtained,as shown in Fig.5.The collision velocities and collision angles of the 11 gauges points were represented by dotted lines in different colors.

    Fig.5.Weldability window of TA1/Q235 explosive welding.

    It could be seen in Fig.4 that the first gauges point was located at the edge of the weldability window,and the following gauges points were in the middle of the window.The lower collision velocity at the initiating end would affect the interfacial bonding of clad plate.

    3.2.Collision simulation results

    TA1/Q235 explosive welding was simulated by the welding parameters of the 11 groups in Table 9,and the results were shown in Fig.6.

    The collision velocity of the first group was low,and the interface exhibited a linear bonding.From the second group to the next ten groups,as the detonation transmission distance increased,the collision velocity gradually stabilized,and the bonding interface transformed from straight to wavy.There were scattered particles in the collision zone,which were metal jets of titanium and steel.The number of titanium particles were significantly more than that of steel particles.Materials with low density were more likely to form jets,which was consistent with the results of Wang [42].Metal jet could remove oxide layer and impurities on the inner surface of base and flyer layers,which was beneficial to the bonding of the two materials.

    3.3.Microscopic morphology analysis

    In order to study the morphology of TA1/Q235 bonding interface,the metallographic sample was prepared by grinding and polishing the sample along the direction parallel to the detonation wave.The microstructure was observed by OM,as shown in Fig.7.

    Fig.7.Metallographic structure of TA1/Q235 interface.

    Fig.7 showed' the metallographic structure of TA1/Q235 clad plate.A black molten metal appeared at the interface,which was mainly bonded in the form of molten layer,and the grains near the interface were streamlined.During explosive welding,the high speed collision in a very short time caused the melting of the interfacial metal and strong plastic deformation of the grains on the steel side,resulting in rheological phenomenon and the grains on the steel side exhibited a streamline shape.The phenomenon was accordance with previous works [43-45].The interfacial air was not completely discharged in the high speed collision between base and flyer layers.Under the joint action of adiabatic compression heat and plastic deformation heat,the interfacial metals melted and diffused to form a black molten layer [44].

    It could be seen in Fig.7 that the metallographic structure in the vortex of the crest contained Ti metal particles.Part of the broken particles were involved in the vortex during the movement,and finally formed molten blocks coated by base material.It was consistent with the phenomenon observed in the explosive welding by predecessors [11,46,47].

    In order to further study,the components of the molten block in the vortex and molten layer at the crest,SEM observation and EDS analysis were performed,and the results were shown in Fig.8.

    Fig.8.SEM and EDS analysis of the TA1/Q235 clad plate:(a)waveform at the interface;(b)Point scanning at the crest;(c)Map scanning at the crest;(d)Partial magnification of the molten region at the crest.

    Fig.8(a) showed the back scattering diagram of the TA1/Q235 bonding interface.The average wavelength and amplitude were 100 μm and 35 μm,respectively.No holes and cracks appeared at the interface,indicating that the TA1/Q235 clad plate had good bonding quality.The average thickness of titanium layer was 170 μm,lower than its original thickness of 200 μm.Because the residual energy of the collision between base and flyer layers directly was acted on the metallic material,the residual deformation occurred in the thickness of the clad plate [19,40].Fig.8(b)displayed the local magnified scanning electron microscopy image of the wave crest.Molten layer exited on the TA1/Q235 bonding surface and the vortex of the crest contained molten block.Point scanning was conducted for points 1 to 6 in Fig.8(b)to analyze the components of molten layer and molten block,and the results were shown in Table 11.According to the point scanning element analysis of points 1 to 3,the molten layer was mainly composed of Ti element and contained a small amount of Fe and O elements.It could be seen in Table 11 that O element was detected in the molten layer,which might be because the inner surface of the metallic plate was not completely cleaned or the air between flyer and base plates was not completely expelled [5,48].According to the atom ratio of Ti to Fe,the molten block was mainly composed of intermetallic compounds of FeTi and Fe2Ti [7,10,12].

    Table 11 Point scanning analysis results.

    It could be observed in Fig.8(c) and (d) that the tissues on the steel side rotated,and the metallic particles in the middle form vortices,reflecting the characteristics of rotational motion during the formation of the wavy interface.It was consistent with the grain deformation of steel in the metallographic observation,indicating that the interfacial metal was in a state of high temperature and high pressure in the process of explosive welding,and the metal exhibited quasi-fluid behavior [18,19].The molten titanium and oxygen elements might form a small amount of titanium oxides,while a small amount of Fe elements diffused to the titanium layer near the interface.The molten metal cooled in a very short time,thus elemental diffusion was not obvious.

    3.4.Mechanical property testing

    The tensile and bending specimens were prepared following GB/T 6396-2008,which was used to characterize the bonding strength of the interface under tensile failure and the plastic deformation ability of the clad plate under bending load.The tensile and bending specimens were processed by three-point bending and tensile tests,respectively.The thickness of tensile and bending specimens was 2 mm,including 200 μm thick titanium layer and 1.8 mm thick steel layer.The specific sizes were shown in Fig.9 and Fig.10.

    Fig.9.The size of tensile specimen.

    Fig.10.The size of bending specimen.

    The specimens were put into the three-point bending mold for bending test,and the bending specimen was observed for separation or crack to characterize its cold working bending performance.Experimental conditions and results were shown in Table 12 and Fig.11,respectively.

    Fig.11.Physical drawing of specimen after bending.

    Table 12 Conditions and results of bending test.

    It could be seen from Table 12 and Fig.11 that no separation or local cracks were found at the interface of outcurve and incurve specimens,and the interface remained intact,indicating that the clad plates had good bending properties during cold working.

    There might be microscopic defects at the bonding interface of the clad plate,and these defects might develop along the welding direction as crack sources under the action of external loading.The fracture morphology was observed by SEM to study interfacial morphology and bonding quality of tensile fracture specimens.The tensile failure specimen and fracture morphology were shown in Fig.12 and Fig.13,respectively.

    Fig.12.Physical drawing of tensile failure specimen.

    Fig.13.Fractography of tensile fracture specimen close to the interface: (a) At the interface;(b) TA1 layer;(c) Q235 layer.

    Fig.13 showed the fractography of titanium foil/steel tensilefailure specimen.No separation and cracks were observed at the fracture interface,and the bonding quality of the interface was good.The tensile fracture exhibited obvious plastic deformation,and there were numerous dimples with different sizes on the fracture surface of titanium and steel layers.Compared with that of the titanium side,the dimple size on the steel side was smaller and shallower,as shown in Fig.13(b) and Fig.13(c).After high speed collision,high temperature melting and rapid cooling occurred at the interface [11].Although the process restored the toughness of the material to some extent,the possible microscopic holes in the material could be not eliminated.After nucleation,growth and aggregation of microspores under plastic deformation,these microspores were connected to each other,resulting in the ductile fracture of the material [5,48].

    3.5.Formation mechanism of waveform and molten block

    Explosive welding is transient and it is difficult to study the whole welding process through experiment.Bahrani-blackcrossland theory,helmholtz instability theory,vortex shedding mechanism and stress wave mechanism are the main theoretical achievements at present,among which Bahrani-black-crossland theory has a high degree of recognition.The theory takes into account the effects of collision point pressure,jet penetration and shear stress,which describes the formation of vortices and periodic waveforms vividly [18,49].

    The parameters of collision velocity of 1358 m/s and collision angle of 2°were used for the collision simulation.The particles that constituted the waveform were tracked,and their velocity vectors at each stage were shown in Fig.14.The observation position was fixed and the variation of interfacial waveform was recorded every 0.01 μs,as shown in Fig.14(a).The observed interfacial wave crest moved 200 μm from the beginning to the final formation.Therefore,when the collision velocity was appropriate,the interface still needed a certain distance to form wavy bonding,which might affect the bonding morphology at the initiation point.The simulation and velocity vector diagrams of key positions of explosive welding interface were studied,as shown in Fig.14(b)-Fig.14(f).In the Bahrani-black-crossland theory,it was considered that the interface presented wavy bonding under the action of salient and re-entrant jets [49].

    Fig.14.Collision simulation diagrams and velocity vector diagram: (a) The changing process of waveform formation,The steps of interfacial waveform formation (b1-d1)with corresponding velocity vector (b2-d2),The beginning of the vortex (e1) with corresponding velocity vector (e2),(f) The end of the vortex.

    Fig.14(b1) showed the initial position of the interfacial waveform.It could be seen that the salient jet generated by the previous waveform scoured base material.The jet resulted in indentation and bump on the surface of base material,which gradually developed into a complete waveform in the subsequent evolution.The velocity of the re-entrant jet reached about 2000 m/s.The waveform formed under the action of high speed scouring and extrusion indicated the important role of jet on the formation of interfacial wave.The salient jet collided with the wave crest and formed reentrant jet in front of wave crest,as shown in Fig.14(c1) and Fig.14(d1).The direction of re-entrant jet was gradually downward,creating conditions for the formation of the next waveform(Fig.14(d1)).As the collision point moved,the particle velocity of the interfacial wave slowed down gradually.At this time,the reentrant jet was easy to form defects such as vortices and holes(Fig.14(e1)),which could affect the bonding performance[11,21,44,50].The re-entrant jet was composed of molten steel and titanium at high temperature,and the air at the interface was not discharged in time,providing an environment for Fe and Ti elements to form metal oxides and intermetallic compounds at high temperature(Fig.14(f)).

    In the collision simulation study,vortex simulation diagram of TA1/Q235 explosive welding could be obtained,as shown in Fig.15(a).The molten block was composed of steel and titanium elements.This was because that steel and titanium melted in a high speed collision,resulting in mutual diffusion and the formation of intermetallic compounds.It could be seen in Fig.15(a)that the gap between particles was large,and there might be oxygen not completely expelled in time at the collision interface,resulting in the formation of metal oxides at the interface.It was similar to the component of molten block observed by SEM image in Fig.15(b).

    Fig.15.SEM and simulation images of vortex: (a) Simulation image of vortex;(b) SEM image of vortex.

    3.6.Interfacial characteristic of TA1/Q235 explosive welding

    The plastic strain,density,temperature and pressure variation rules of collision interface were obtained by numerical simulation to study the interfacial characteristic,as shown in Fig.16.

    Fig.16.Interfacial characteristic diagrams of explosive welding: (a) Temperature distribution;(b) Pressure distribution;(c) Density distribution;(d) Plastic strain distribution.

    Fig.16(a)-Fig.16(d)showed the temperature,pressure,density and effective plastic strain distributions of TA1/Q235 explosive welding interface,respectively.The temperature of the interface and vortex was close to 4000 K,and the interfacial pressure basically exceeded 18 GPa.As the distance from the interface increased,the temperature and pressure of base and flyer materials decreased rapidly.Both base and flyer materials melted,and intermetallic compounds were easily formed at the bonding interface [7,10,12].The molten layer at the interface was usually thin,and base and flyer materials still maintained good mechanical properties when the distance from the interface was 50 μm.The density of titanium and steel was 4.5 g/cm3and 8.0 g/cm3,respectively.However,the density of molten layer at the interface was 7.0 g/cm3,which was between that of titanium and steel.The interfacial metal melted under the action of high temperature and high pressure generated by high speed collision.The molten metal cooled in a very short time to form molten layer,and created conditions for the generation of intermetallic compounds[10,18].It was consistent with the SEM observation.The maximum effective plastic strain of the molten layer and the molten block in the vortex reaches 6.Generally,the higher the temperature was,the lower the strength of the metal was,and the pressure was sharply reduced as the distance from the interface increased [51].Therefore,the effective plastic strain value of the metal at the interface was much larger than that of materials far away from the interface.

    4.Conclusions

    The explosive welding of 200 μm thick titanium foil to steel plate was studied by numerical simulation and experiment.Optical microscope(OM),scanning electron microscope(SEM)and energy disperse spectroscopy (EDS) were used to observe the interfacial microscopic morphology of the TA1/Q235 clad plate.Smoothed particle hydrodynamics(SPH)simulation method code was used to study the forming mechanism of waveform and vortex,and the following conclusions could be obtained:

    (1) Salt was used as a pressure transfer layer,which could decrease the acceleration process of explosive welding and avoid the high temperature burn caused by explosive detonation,and titanium foil/steel explosive welding was successfully achieved.No separation or local cracks were found at the interface of bending and tensile fracture specimens,and the interface remained intact,indicating that the clad plate exhibited good cold workability.

    (2) Regular waveforms could be formed at the interface of the TA1/Q235 clad plate.The average thickness of the titanium layer was 170 μm,and the average wavelength and amplitude of the interfacial waveform were 100 μm and 35 μm,respectively.

    (3) The interface of titanium foil/steel clad plate was mainly bonded in the form of molten layer.The molten layer was mainly composed of Ti element,containing a small amount of Fe element.There were molten blocks in the vortex of wave crest.According to the atomic ratio,the intermetallic compounds were mainly composed of FeTi and Fe2Ti.

    (4) The re-entry jet resulted in indentation and bump on the surface of base material,which gradually developed into a complete waveform in the subsequent evolution,indicating the important role of jet on the formation of interfacial waveform.

    Declaration of competing interest

    The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

    欧美一区二区国产精品久久精品| 午夜亚洲福利在线播放| 久久久久久久久大av| 边亲边吃奶的免费视频| 国产毛片a区久久久久| 色5月婷婷丁香| 黄色欧美视频在线观看| 亚洲欧美精品综合久久99| 日韩一区二区三区影片| 亚洲在线自拍视频| 全区人妻精品视频| 免费av毛片视频| 一个人观看的视频www高清免费观看| 国产麻豆成人av免费视频| 99久久成人亚洲精品观看| 日韩国内少妇激情av| 91久久精品电影网| 久久精品影院6| 亚洲欧美清纯卡通| 精品久久久久久久久久久久久| 伊人久久精品亚洲午夜| av播播在线观看一区| 狂野欧美激情性xxxx在线观看| 国产片特级美女逼逼视频| 丝袜喷水一区| 99视频精品全部免费 在线| 亚洲欧洲国产日韩| 欧美zozozo另类| 婷婷色av中文字幕| 国产午夜精品论理片| 男人舔奶头视频| 少妇的逼好多水| 一本一本综合久久| 国产日韩欧美在线精品| 日本黄色视频三级网站网址| 最近最新中文字幕免费大全7| 天天躁日日操中文字幕| 亚洲图色成人| 国语自产精品视频在线第100页| 日韩中字成人| 岛国在线免费视频观看| 51国产日韩欧美| 欧美色视频一区免费| 99视频精品全部免费 在线| 国内精品一区二区在线观看| 国产精品一区二区性色av| 亚洲精品乱码久久久v下载方式| 国产探花在线观看一区二区| 国产午夜福利久久久久久| 国产成人免费观看mmmm| 日本一二三区视频观看| 国产高清三级在线| 精品熟女少妇av免费看| 国产精品一区二区三区四区久久| 男人和女人高潮做爰伦理| 99热这里只有是精品50| 精品熟女少妇av免费看| 又粗又硬又长又爽又黄的视频| 国产亚洲av嫩草精品影院| 真实男女啪啪啪动态图| 国产极品精品免费视频能看的| 26uuu在线亚洲综合色| 亚洲电影在线观看av| 国产乱来视频区| 亚洲欧美中文字幕日韩二区| 2021少妇久久久久久久久久久| 国产高清国产精品国产三级 | 久久鲁丝午夜福利片| 精品人妻视频免费看| 日韩成人av中文字幕在线观看| 啦啦啦啦在线视频资源| 久久久久国产网址| 亚洲美女视频黄频| 一边摸一边抽搐一进一小说| 最近最新中文字幕大全电影3| 亚洲国产高清在线一区二区三| 亚州av有码| 在现免费观看毛片| 国产激情偷乱视频一区二区| 2022亚洲国产成人精品| 久久综合国产亚洲精品| 18禁动态无遮挡网站| 精品酒店卫生间| 精品国产三级普通话版| 一区二区三区免费毛片| 亚洲在线自拍视频| 又粗又爽又猛毛片免费看| 丰满乱子伦码专区| 色视频www国产| 天天一区二区日本电影三级| 久久亚洲精品不卡| 18禁裸乳无遮挡免费网站照片| 国产大屁股一区二区在线视频| 欧美日韩一区二区视频在线观看视频在线 | 日日摸夜夜添夜夜爱| 少妇猛男粗大的猛烈进出视频 | 又粗又硬又长又爽又黄的视频| av在线播放精品| 免费大片18禁| 狠狠狠狠99中文字幕| 亚洲av电影在线观看一区二区三区 | 亚洲av电影不卡..在线观看| 日韩在线高清观看一区二区三区| 村上凉子中文字幕在线| 欧美激情在线99| 在线播放国产精品三级| 熟女电影av网| 精品久久国产蜜桃| 啦啦啦啦在线视频资源| 大香蕉久久网| 亚洲精品乱久久久久久| 乱系列少妇在线播放| 国产精品人妻久久久久久| 亚洲精品日韩在线中文字幕| 岛国在线免费视频观看| 高清在线视频一区二区三区 | 天天躁日日操中文字幕| 亚洲av成人精品一区久久| 午夜福利网站1000一区二区三区| 91久久精品国产一区二区三区| 啦啦啦啦在线视频资源| 国产精品一区二区在线观看99 | 噜噜噜噜噜久久久久久91| 麻豆av噜噜一区二区三区| 亚洲最大成人中文| 七月丁香在线播放| 能在线免费观看的黄片| 麻豆成人av视频| 欧美bdsm另类| 一区二区三区乱码不卡18| 午夜精品一区二区三区免费看| 久久久久久九九精品二区国产| 狂野欧美激情性xxxx在线观看| 免费看日本二区| 白带黄色成豆腐渣| 五月玫瑰六月丁香| 成年免费大片在线观看| 国产精品1区2区在线观看.| 丰满人妻一区二区三区视频av| 日韩亚洲欧美综合| 亚洲成av人片在线播放无| 3wmmmm亚洲av在线观看| 亚洲精品国产av成人精品| 联通29元200g的流量卡| 国产 一区精品| 日韩欧美精品免费久久| 国产激情偷乱视频一区二区| 婷婷色综合大香蕉| 能在线免费看毛片的网站| 久久久精品大字幕| 亚洲乱码一区二区免费版| 一个人观看的视频www高清免费观看| 久久久a久久爽久久v久久| 国产精品综合久久久久久久免费| 在线观看美女被高潮喷水网站| 九九爱精品视频在线观看| 午夜福利在线观看免费完整高清在| 国产一区二区在线av高清观看| 国产69精品久久久久777片| 国产白丝娇喘喷水9色精品| 亚洲一级一片aⅴ在线观看| 毛片女人毛片| 国产 一区 欧美 日韩| 久久久久久久久久黄片| 国产私拍福利视频在线观看| 最近中文字幕高清免费大全6| 国产精品永久免费网站| 大又大粗又爽又黄少妇毛片口| 插逼视频在线观看| 国产高清国产精品国产三级 | 3wmmmm亚洲av在线观看| 老司机影院成人| 伦精品一区二区三区| 亚洲怡红院男人天堂| 成人性生交大片免费视频hd| 免费看光身美女| 日日撸夜夜添| 三级国产精品片| 老司机影院毛片| 麻豆国产97在线/欧美| 91精品国产九色| 国产熟女欧美一区二区| 18禁在线播放成人免费| 十八禁国产超污无遮挡网站| 亚洲乱码一区二区免费版| 丰满少妇做爰视频| 亚洲精华国产精华液的使用体验| 亚洲伊人久久精品综合 | 午夜福利在线观看免费完整高清在| 亚洲最大成人av| 内地一区二区视频在线| 日韩av不卡免费在线播放| 一二三四中文在线观看免费高清| 国产免费又黄又爽又色| 日本色播在线视频| 国产片特级美女逼逼视频| 天天一区二区日本电影三级| 欧美精品国产亚洲| 国产精品蜜桃在线观看| 三级国产精品欧美在线观看| 久久精品久久精品一区二区三区| 又黄又爽又刺激的免费视频.| 国产精品福利在线免费观看| 春色校园在线视频观看| 91狼人影院| 色吧在线观看| 久久久久性生活片| 亚洲经典国产精华液单| 国国产精品蜜臀av免费| 精品99又大又爽又粗少妇毛片| av在线蜜桃| 日韩成人av中文字幕在线观看| 一级爰片在线观看| 黄片wwwwww| 欧美色视频一区免费| 看免费成人av毛片| 久久久久久大精品| 老师上课跳d突然被开到最大视频| 亚洲精品自拍成人| 能在线免费看毛片的网站| 亚洲国产日韩欧美精品在线观看| 国产精品一及| 女人被狂操c到高潮| 亚洲国产高清在线一区二区三| 免费观看人在逋| 午夜精品一区二区三区免费看| 婷婷色综合大香蕉| 最近的中文字幕免费完整| 网址你懂的国产日韩在线| 色综合站精品国产| 精品人妻一区二区三区麻豆| 亚洲成人精品中文字幕电影| 欧美色视频一区免费| 少妇高潮的动态图| 色综合站精品国产| 超碰97精品在线观看| 夜夜爽夜夜爽视频| 国产亚洲av嫩草精品影院| 亚洲丝袜综合中文字幕| 赤兔流量卡办理| 高清午夜精品一区二区三区| 亚洲精品,欧美精品| 成人特级av手机在线观看| 精品久久久久久成人av| 国内少妇人妻偷人精品xxx网站| 国产成人a∨麻豆精品| 国产亚洲精品av在线| 国产精品国产三级国产av玫瑰| 少妇人妻一区二区三区视频| 日本免费a在线| 国产色爽女视频免费观看| 91aial.com中文字幕在线观看| 99久国产av精品国产电影| 熟妇人妻久久中文字幕3abv| 男人狂女人下面高潮的视频| 在线a可以看的网站| 国产精品,欧美在线| 国产精品一二三区在线看| 国产精品国产高清国产av| 国产亚洲午夜精品一区二区久久 | 久久午夜福利片| 国产午夜精品论理片| АⅤ资源中文在线天堂| videos熟女内射| 黄片无遮挡物在线观看| 久久精品夜色国产| 国产成人精品久久久久久| 女人十人毛片免费观看3o分钟| 一级毛片aaaaaa免费看小| 搡女人真爽免费视频火全软件| 狂野欧美白嫩少妇大欣赏| 日本黄色视频三级网站网址| 亚洲高清免费不卡视频| 天天一区二区日本电影三级| 乱人视频在线观看| 国产激情偷乱视频一区二区| 亚洲18禁久久av| 中文字幕免费在线视频6| 亚洲av中文av极速乱| 国产在视频线精品| h日本视频在线播放| 成人漫画全彩无遮挡| 可以在线观看毛片的网站| 日韩制服骚丝袜av| 国产精品久久久久久久久免| 日本与韩国留学比较| 99在线视频只有这里精品首页| 一级黄色大片毛片| 男女视频在线观看网站免费| 一个人看视频在线观看www免费| 九色成人免费人妻av| 国产亚洲av片在线观看秒播厂 | 亚洲一级一片aⅴ在线观看| 亚洲av不卡在线观看| 亚洲精品久久久久久婷婷小说 | 波野结衣二区三区在线| 国产黄片视频在线免费观看| 麻豆成人av视频| 97在线视频观看| 丝袜喷水一区| 高清日韩中文字幕在线| av线在线观看网站| 色噜噜av男人的天堂激情| 欧美丝袜亚洲另类| 日韩精品青青久久久久久| 午夜福利视频1000在线观看| .国产精品久久| av在线播放精品| 色5月婷婷丁香| 久久久久久久午夜电影| 久久久久久久亚洲中文字幕| 高清日韩中文字幕在线| 又爽又黄a免费视频| 五月伊人婷婷丁香| 欧美成人精品欧美一级黄| 日产精品乱码卡一卡2卡三| 简卡轻食公司| 成人毛片a级毛片在线播放| 禁无遮挡网站| av.在线天堂| 18禁在线无遮挡免费观看视频| 日韩,欧美,国产一区二区三区 | 国产熟女欧美一区二区| 亚洲国产最新在线播放| 国产精品1区2区在线观看.| 女人十人毛片免费观看3o分钟| 欧美+日韩+精品| 久久久久久大精品| 久久久欧美国产精品| 99在线人妻在线中文字幕| 99久久人妻综合| 精华霜和精华液先用哪个| 欧美丝袜亚洲另类| 欧美日本亚洲视频在线播放| 国产亚洲一区二区精品| 亚洲成人精品中文字幕电影| 久久精品国产99精品国产亚洲性色| 欧美又色又爽又黄视频| 午夜激情欧美在线| 2022亚洲国产成人精品| 国产精品国产三级国产专区5o | 国产精品久久电影中文字幕| 国内揄拍国产精品人妻在线| 日本三级黄在线观看| 欧美日韩精品成人综合77777| 成人鲁丝片一二三区免费| 亚洲真实伦在线观看| 亚洲人与动物交配视频| 午夜日本视频在线| 免费黄色在线免费观看| 只有这里有精品99| 日本黄色片子视频| 中文欧美无线码| 麻豆乱淫一区二区| 国产精品福利在线免费观看| 亚洲精品456在线播放app| 亚洲乱码一区二区免费版| 桃色一区二区三区在线观看| 国产精品无大码| 亚洲一区高清亚洲精品| 国产一区二区三区av在线| 国产视频内射| 深夜a级毛片| 免费看日本二区| 国产 一区精品| 久久久国产成人精品二区| av在线观看视频网站免费| 韩国av在线不卡| 亚洲激情五月婷婷啪啪| 国产精品国产三级国产专区5o | 国产乱人偷精品视频| 国产精品久久久久久精品电影| 国产精品永久免费网站| 亚洲一级一片aⅴ在线观看| 丝袜喷水一区| 少妇的逼好多水| 欧美潮喷喷水| 成人特级av手机在线观看| 人人妻人人看人人澡| 亚洲最大成人av| 国产亚洲精品av在线| 99九九线精品视频在线观看视频| 国产精品乱码一区二三区的特点| 女人十人毛片免费观看3o分钟| 国产毛片a区久久久久| 少妇猛男粗大的猛烈进出视频 | 免费看光身美女| 91在线精品国自产拍蜜月| 国产成人freesex在线| 搡老妇女老女人老熟妇| 精品酒店卫生间| 欧美成人a在线观看| 免费av不卡在线播放| 两个人视频免费观看高清| 日本熟妇午夜| 国产精品久久久久久av不卡| 欧美激情久久久久久爽电影| 床上黄色一级片| 少妇人妻精品综合一区二区| 插阴视频在线观看视频| 观看免费一级毛片| 欧美三级亚洲精品| 天美传媒精品一区二区| 伊人久久精品亚洲午夜| 我要看日韩黄色一级片| 国产精品不卡视频一区二区| 日日干狠狠操夜夜爽| 黄色一级大片看看| 最后的刺客免费高清国语| 精品国产一区二区三区久久久樱花 | 精品人妻熟女av久视频| av播播在线观看一区| 晚上一个人看的免费电影| 国产精品av视频在线免费观看| 亚洲天堂国产精品一区在线| 中文精品一卡2卡3卡4更新| 成人综合一区亚洲| 舔av片在线| 伊人久久精品亚洲午夜| 成人无遮挡网站| 国产精品久久久久久久电影| 午夜爱爱视频在线播放| 亚洲自拍偷在线| 亚洲人成网站在线播| 国产成人免费观看mmmm| 国产一区有黄有色的免费视频 | 国产极品精品免费视频能看的| 国产男人的电影天堂91| 97热精品久久久久久| av专区在线播放| 国产私拍福利视频在线观看| 午夜久久久久精精品| 精品人妻视频免费看| 午夜福利视频1000在线观看| 久久精品国产亚洲av涩爱| 男女国产视频网站| 久久鲁丝午夜福利片| 18禁在线无遮挡免费观看视频| 久久精品91蜜桃| 精品人妻熟女av久视频| 99热网站在线观看| 亚洲天堂国产精品一区在线| 亚洲欧洲日产国产| 日韩国内少妇激情av| 嫩草影院入口| 1000部很黄的大片| 成人鲁丝片一二三区免费| 精品国产三级普通话版| 日韩视频在线欧美| 超碰av人人做人人爽久久| 久久久久久久久久久免费av| 2021少妇久久久久久久久久久| 国产精品综合久久久久久久免费| 麻豆av噜噜一区二区三区| 欧美bdsm另类| 亚洲av成人精品一区久久| 色综合站精品国产| 亚洲最大成人中文| 男人的好看免费观看在线视频| 身体一侧抽搐| 日韩一区二区三区影片| 亚洲欧洲国产日韩| 啦啦啦观看免费观看视频高清| 综合色av麻豆| 黄色配什么色好看| 国产精华一区二区三区| 波多野结衣高清无吗| 中文字幕制服av| 国产精品一及| 国产成人午夜福利电影在线观看| 卡戴珊不雅视频在线播放| 午夜福利在线观看免费完整高清在| 日韩 亚洲 欧美在线| 日韩欧美精品v在线| 日本三级黄在线观看| 久久人人爽人人爽人人片va| 搞女人的毛片| 丰满少妇做爰视频| 亚洲精品日韩在线中文字幕| 内地一区二区视频在线| 国产国拍精品亚洲av在线观看| 日韩成人伦理影院| 能在线免费看毛片的网站| 两个人的视频大全免费| 久久草成人影院| 久久99热这里只有精品18| 亚洲人成网站高清观看| av在线天堂中文字幕| 三级经典国产精品| 精品一区二区三区视频在线| av免费观看日本| av在线老鸭窝| 舔av片在线| 国产精品1区2区在线观看.| 久久久国产成人免费| 中文欧美无线码| 级片在线观看| 久久久精品94久久精品| 人妻制服诱惑在线中文字幕| 男人和女人高潮做爰伦理| 久久精品人妻少妇| 晚上一个人看的免费电影| 日韩三级伦理在线观看| 欧美日韩国产亚洲二区| 最后的刺客免费高清国语| 午夜日本视频在线| 亚洲国产精品国产精品| 国产精品爽爽va在线观看网站| 看十八女毛片水多多多| 成人av在线播放网站| 欧美日韩精品成人综合77777| 一级爰片在线观看| 国产黄色小视频在线观看| 亚洲国产高清在线一区二区三| 久久精品国产亚洲网站| 精品一区二区免费观看| 欧美高清成人免费视频www| 免费搜索国产男女视频| 边亲边吃奶的免费视频| 午夜精品国产一区二区电影 | 我的老师免费观看完整版| 国产精品一二三区在线看| 久久久久久久久大av| 国产午夜精品一二区理论片| 嫩草影院入口| 久久欧美精品欧美久久欧美| 欧美高清性xxxxhd video| 国产黄a三级三级三级人| 日韩,欧美,国产一区二区三区 | 汤姆久久久久久久影院中文字幕 | 国产成人a区在线观看| 亚洲av一区综合| 精品熟女少妇av免费看| 亚洲精品456在线播放app| av又黄又爽大尺度在线免费看 | 国产精品爽爽va在线观看网站| 免费无遮挡裸体视频| 精品人妻熟女av久视频| 看非洲黑人一级黄片| 久久久久久久亚洲中文字幕| 少妇裸体淫交视频免费看高清| 欧美日韩一区二区视频在线观看视频在线 | 中文欧美无线码| 老师上课跳d突然被开到最大视频| 国产精品日韩av在线免费观看| www.av在线官网国产| 精品一区二区三区视频在线| 久久久久精品久久久久真实原创| 久久这里有精品视频免费| 毛片一级片免费看久久久久| 亚洲激情五月婷婷啪啪| av黄色大香蕉| 亚洲av电影在线观看一区二区三区 | 99久久成人亚洲精品观看| 我要看日韩黄色一级片| 久久精品91蜜桃| 国产v大片淫在线免费观看| 国产国拍精品亚洲av在线观看| 少妇高潮的动态图| 午夜激情福利司机影院| 我的女老师完整版在线观看| 91狼人影院| 久久久色成人| 26uuu在线亚洲综合色| 赤兔流量卡办理| 能在线免费看毛片的网站| 亚洲欧美精品专区久久| 免费观看精品视频网站| 天天躁日日操中文字幕| av在线观看视频网站免费| 久久久久久久亚洲中文字幕| 国产高清有码在线观看视频| 国产精品综合久久久久久久免费| 日本三级黄在线观看| 亚洲av电影在线观看一区二区三区 | 又黄又爽又刺激的免费视频.| 日本av手机在线免费观看| 成人毛片a级毛片在线播放| 直男gayav资源| 免费大片18禁| 日韩欧美 国产精品| 国产久久久一区二区三区| 欧美性猛交╳xxx乱大交人| 免费观看在线日韩| 一卡2卡三卡四卡精品乱码亚洲| 久久久精品94久久精品| 夜夜看夜夜爽夜夜摸| 特大巨黑吊av在线直播| 久久精品综合一区二区三区| 中文亚洲av片在线观看爽| 蜜桃亚洲精品一区二区三区| 国产黄a三级三级三级人| 成人亚洲欧美一区二区av| 欧美3d第一页| 国产精品三级大全| 国产av码专区亚洲av| 特大巨黑吊av在线直播| 综合色av麻豆| 国产成人精品久久久久久| 三级国产精品片| 国内揄拍国产精品人妻在线| 老司机福利观看| 亚洲人成网站在线观看播放| 国产精品精品国产色婷婷| 日韩,欧美,国产一区二区三区 | 亚洲人成网站在线观看播放| 免费观看人在逋| 夫妻性生交免费视频一级片| 国产老妇伦熟女老妇高清| 色综合色国产| 99久久精品国产国产毛片| 亚洲激情五月婷婷啪啪| 一卡2卡三卡四卡精品乱码亚洲| 亚洲自偷自拍三级| 日韩成人伦理影院|