    Inherent relationship between process parameters,crystallization and mechanical properties of continuous carbon fiber reinforced PEEK composites

    2023-07-04 08:00:06XiolongLihuWenShiyuWngJinyouXioWenhoLiXioHou
    Defence Technology 2023年6期

    Xio-long M , Li-hu Wen , Shi-yu Wng ,*, Jin-you Xio , Wen-ho Li , Xio Hou

    a School of Astronautics, Northwestern Polytechnical University, Xi'an, 710072, China

    b China Aerospace Science and Technology Corporation, Beijing,100048, China

    Keywords:Polymer matrix composites Thermoplastic Processing parameters Mechanical properties Crystallization

    ABSTRACT

    1. Introduction

    In recent years, high-performance thermoplastic composites have been successfully applied in the aircraft industries because they exhibit numerous advantages, such as excellent specific stiffness, high toughness and ductility, outstanding thermal stability(PEEK is exceeding 300?C), and shorter manufacturing cycles, etc[1—10]. In particular, thermoplastic composites have excellent impact resistance, corrosion resistance, and high service temperature, which have attracted the attention of military applications before commercial use and have been widely used in military aircraft [11—13]. However, due to the long molecular chain structure of thermoplastic resins such as PEEK and PPS, the high viscosity of the molten resin made it difficult to fully infiltrate the fibers [14—18]. And thermoplastic resin contains amorphous domains and crystallites, which can convert to each other upon temperature change or shear flow [19]. Therefore, the molding process conditions can significantly affect the performance of the thermoplastic composites. In addition, thermoplastic resins have high melting temperatures and a narrow processing window.These harsh conditions have brought considerable challenges to the molding process of high-performance thermoplastic composites.Therefore, it is necessary to optimize the molding processing of thermoplastic composites.

    Different molding processing parameters significantly affect the mechanical properties of thermoplastic composites. A number of researchers have studied the influence of molding processing parameters on mechanical properties [20—26]. Fujihara K et al. [20]optimized the molding temperature and holding time of continuous CF/PEEK composite laminates with bending performance as an indicator,and it was pointed out that excessively high molding temperature and too long holding time would lead to degradation of PEEK and reduce mechanical properties. Similarly,Xu Z et al. [22] found that when CF/PEEK composites via the wrapped yarn method were held at higher molding temperatures(above 420?C) for an excessive time (above 60 min), would have decreased mechanical properties due to matrix degradation.Zheng B et al.[23]investigated the influence of molding temperature and molding pressure on the properties of woven CF/PEEK composites,and pointed out that the optimal process conditions for bending performance were 400?C and 5 MPa, while the molding pressure had little effect on interlaminar shear strength (ILSS). Dai G et al.[24]took the ILSS as the optimization objective,studied the effects of molding temperature,molding pressure,and holding time on the mechanical properties of CF/PEEK cross-ply laminates,and pointed out that the optimal molding conditions were holding time of at least 20 min and molding temperature should be between 400 and 420?C. The current research mostly phenomenologically established the relationship between the molding process parameters such as molding temperature, pressure, and holding time and the macro-mechanical properties. However, these conclusions did not deeply clarify the regulation mechanism of the processing parameters on the macro-mechanical properties of thermoplastic composites.In addition,the viscosity of the molten thermoplastic resin is affected by factors such as the molding temperature and holding time [27]. Therefore, the thermoforming curing processing parameters of thermoplastic composites are not independent of each other but affect each other. However, to the author’s knowledge,there is little information available in the literature about comprehensively and systematically considering the coupling effect of processing parameters on the mechanical properties of thermoplastic composites.

    The mechanical properties of semi-crystalline thermoplastic composites, especially the fracture toughness, were mainly dominated by crystallinity, which was affected by the processing parameters [28—30]. The researchers discussed the effect of processing parameters on the crystallization behavior of thermoplastic resin [31—35]. Yang X and Sun H et al. [33—34] studied the effect of different cooling rates on the non-isothermal crystallization kinetics and discussed the effects of cooling rates on crystal growth and morphology. Gao S L et al. [36] further analyzed the effect of cooling rate on the fracture toughness of thermoplastic composites and revealed the mechanism of cooling rate regulating the fracture toughness of composites by affecting the crystallization process. Processing parameters such as molding temperature,pressure, and holding time also affect crystallization behavior.However, little attention has been devoted to regulating these processing parameters on the crystallization process of thermoplastic composites and their impact on mechanical properties.Therefore,it is of great significance to study the effects of molding temperature, pressure, and holding time on the crystallization of composites and quantitatively discuss the relationship between crystallization and mechanical properties.

    This study aimed to investigate the effects of molding process parameters on molding quality, mechanical properties, and crystallization behavior of continuous CF/PEEK composites. Thus, the CF/PEEK composite laminates were fabricated by three-parameter four-level orthogonal thermoforming process parameters. Threepoint bending test, double cantilever beam (DCB) test, and differential scanning calorimetry (DSC) test were carried out to analyze the effects of the molding process parameters (molding temperature, molding pressure, and holding time) on the mechanical properties and crystallization behavior of the CF/PEEK composites.The molding quality and failure mechanism were investigated by microscopic morphologies of the CF/PEEK specimen.The effects of processing conditions on fiber/resin interaction and crystallization of CF/PEEK composites were systematically discussed, and the mechanism of the effect of matrix crystallization on the mechanical properties of the composites was studied.

    2. Materials and fabrication

    The material used unidirectional PEEK-carbon prepreg commercialized by VICTREX, which has a melting temperature of 343?C and a fiber mass fraction of 54%. For this study, CF/PEEK composite laminates were fabricated using the thermoforming method. The CF/PEEK composite laminates of 2 mm nominal thickness were hand lay-up of 16 plies of unidirectional prepreg,which were consolidated in a matching steel mold.A pre-crack was created by laying a 16 μm thick polyimide high-temperature resistant film on the middle plane, which was coated with a release agent.

    The determination of processing parameters was closely related to the fluidity of the resin. According to the relationship between the viscosity of PEEK and the processing conditions [27], the viscosity of PEEK in the molten state was not only related to molding temperature but also affected by holding time,as shown in Fig.1.In addition,considering the degradation of the PEEK matrix caused by high molding temperature [20,22]. Therefore, this study selected 360—405?C as the molding temperature,10—40 min as the holding time, and designed the three-parameter four-level orthogonal thermoforming process conditions, as shown in Fig. 2. The experimental design process and objectives of this paper were shown in Fig. 3.

    Fig.1. Viscosity of PEEK as a function of time for different temperatures [27].

    Fig. 2. Fabrication conditions of continuous CF/PEEK composite laminates by L16 (43)orthogonal experiments.

    Fig. 3. Experimental design process and objectives.

    Fig. 4. Sketches of specimens and testing fixtures for mechanical characterizations: (a) DCB specimen; (b) Three-point bending specimen.

    3. Characterization methods

    3.1. Mechanical characterization

    In order to characterize the influence of thermoforming process parameters on the mechanical properties of thermoplastic composites, double cantilever beam (DCB) tests and three-point bending tests are carried out through an electromechanical universal testing machine(INSTRON 5569) at room temperature.DCB tests are performed according to the ASTM standard D5528 with a loading speed of 2 mm/min.The nominal size of the DCB specimen with the initial crack length of 50 mm(a0)is 150×25×2 mm3,as shown in Fig.4(a).The digital image correlation(DIC)measurement technique is used for crack extension length measurement,which is recorded using a HIKVISION MV-CA060-11 GM industrial camera(resolution 3072 × 2048, image element size 2.4 μm) with an acquisition framerate of 10 s a piece. Based on the full-field displacement obtained by the DIC measurement system, accurately locate the crack tip position, and obtain the crack extension length in real-time.Regularly track the position of the crack tip and record the applied load and opening displacement at each crack extension. The mode-I interlaminar fracture toughness (GIC) is calculated from Eq. (1) [37].

    wherePis the applied load,δ is the load point displacement,bis the width of a specimen,ais the delamination length, and Δ is the corrective factor for crack length.

    Three-point bending tests according to the ASTM standard D7264 are conducted.The span-to-depth ratio is 32,and the crosshead speed is 1 mm/min. The specimen dimension is 81 × 12 ×2 mm3,as shown in Fig.4(b).The test specimens are cut out of the laminates thermoformed with different processing parameters using a waterjet cutting machine.Moreover,the fracture surfaces of microstructure are observed using the scanning electron microscope (SEM) to study the influence of molding process conditions on crystallization and mechanical properties of CF/PEEK composites.

    3.2. Thermal characterization

    In order to study the crystallization behavior of CF/PEEK laminates under different molding process conditions, differential scanning calorimetry (DSC) is carried out on the Mettler-Toledo DSC machine. The specimen mass is about 10 mg. The DSC tests are heated at a rate of 10?C/min from 25 to 400?C in a nitrogen atmosphere[38].The crystallinity degree(XC)is determined using the following equation [39]:

    whereHfis the melting enthalpy of 100% crystalline PEEK,Hf=130 J/g[40],ΔHmis value of the melting enthalpy,and α is the fiber mass fraction.

    4. Results and discussion

    4.1. Mode-I interlaminar fracture toughness

    4.1.1. The influence of processing parameters on the fracture toughness of CF/PEEK composites

    Fig. 5 illustrates the curves of typical DCB force-displacement andGIC-extended crack length of CF/PEEK specimens fabricated at different molding process conditions. During the load loading process, the interlayer of composites undergoes damage initiation and damage evolution until the load suddenly drops at the peak point and the crack extends. Then the slope of the forcedisplacement curve decreased as the number of crack propagation increased,as shown in Fig.5(a)and Fig.5(b).It is observed that the processing parameters have a significant effect on the crack extension.The load for crack extension increases with the increase of molding temperature and holding time. TheGICof CF/PEEK composites is calculated and plotted in Fig.5(c)and Fig.5(d).It can be clearly found that theGICof CF/PEEK composites increases with increasing molding temperature,pressure and holding time,and a similar trend is proposed in other Ref. [41].

    Fig. 5. Mode-I interlaminar fracture toughness of specimens fabricated at different molding process conditions: (a) Force-displacement curves;(b)Force-displacement curves;(c)GIC-extended crack length curves; (d) GIC-extended crack length curves.

    The relationship between theGICof CF/PEEK composites and the processing parameters is summarized in Fig. 6. In order to more intuitively study the influence of the molding process coupling effect onGIC, the orthogonal test results are interpolated to obtain the contour map of each two processing parameters onGIC, as shown in Fig. 6(b), Fig. 6(c) and Fig. 6(d). From the experimental data in Fig. 6(a), it can be found that the influence of processing parameters on theGICof CF/PEEK composites does not change monotonously, which is reflected in the maximum and minimum values occurring at 375?C,as shown in Fig.6(b).TheGICof CF/PEEK composites results from the coupling effect of various processing parameters. The increase of the molding temperature reduces the viscosity of the resin, and the increase of the molding pressure promotes the permeability of the fiber/matrix, thereby improving the interlayer performance of the composite laminate,as shown in Fig.6(b)and Fig.6(c).Similarly,increasing the molding time allows for better impregnation of the resin with the fibers,improving the fiber/resin bond and thus the mechanical properties, as shown in Fig. 6(d). However, the PEEK matrix evolves over long periods at high temperatures. Chain oxidation and crosslinking are the proposed mechanisms for its thermal degradation, leading to a decrease in the properties and an increase in the viscosity of the PEEK matrix[27], which is detrimental to the impregnation of the fibers with the PEEK matrix.

    Fig.6. Relationship between GIC and molding process parameters of CF/PEEK composites:(a)Orthogonal test results of GIC;(b)Contour map of molding temperature and molding pressure; (c) Contour map of molding pressure and holding time; (d) Contour map of holding time and molding temperature.

    The curves above the contour maps in Fig.6(b)—Fig.6(d)are the trend graphs of the three process parameters onGICaccording to range analysis. It can be seen that the recommended molding process parameters are 405?C, 1.5 MPa, and 40 min with the objective ofGIC. The range analysis results indicate that the influence degree of process parameters onGICis molding pressure,temperature, and holding time in descending order. The detailed analysis is carried out in Section 4.4.

    4.1.2. The influence of processing parameters on the fracture morphology of DCB specimens

    The fracture morphologies of the DCB specimens fabricated at different temperatures and pressures are observed to identify the influence of the processing parameters on the failure mechanism in Fig.7.As shown in Fig.7(a)and Fig.7(b),the exposed fibers and the voids can be clearly seen at the fracture of the specimens. This is mainly due to the poor fluidity of the resin when the molding temperature is low,and the lower molding pressure is not enough to promote penetration of the resin between the fibers,which leads to a weaker bonding interface of the CF/PEEK composites. As the molding temperature and pressure increase, as shown in Fig. 7(c)and Fig.7(d),a large amount of resin residue on the surface of the fiber and a well-bonded fiber/matrix interface can be observed at the fracture of the specimens. These clarify that the fiber/resin forms a strong interfacial bond under high temperature and pressure. More energy is needed for interlaminar crack propagation,and the composite material exhibits higher interlaminar fracture toughness.

    Fig.7. SEM micrographs of the DCB fracture surfaces of specimens fabricated at different molding process conditions:(a)360 ?C,0.25 MPa(40 min);(b)375 ?C,0.5 MPa(20 min);(c) 390 ?C,1 MPa (40 min); (d) 405 ?C,1.5 MPa (20 min).

    The fracture morphologies of the DCB specimens fabricated at different holding times are observed in Fig. 8. As seen in Fig. 8(a)and Fig.8(b),exposed carbon fibers and separate resin clusters are clearly visible on the fracture surface of specimens.This is because the short holding time leads to insufficient infiltration of the resin and fiber. The molten resin is unable to infiltrate the fiber bundles between the different layers, resulting in poor fiber/matrix interface bonding. As the holding time increases, as shown in Fig. 8(c)and Fig. 8(d), the exposed fibers are significantly reduced, and the improved fiber/resin bonding interface can be observed at the fracture of the specimens.These indicate that a longer holding time ensures adequate fiber and resin infiltration and interface strength,thus improving theGICof CF/PEEK composites.

    Fig.8. SEM micrographs of the DCB fracture surfaces of specimens fabricated at different process conditions:(a)10 min(360 ?C,0.5 MPa);(b)20 min(390 ?C,0.25 MPa);(c)30 min(375 ?C,1 MPa); (d) 40 min (405 ?C, 0.5 MPa).

    Fig. 9. Three-point bending typical stress-displacement curves of specimens fabricated at different molding process conditions.

    4.2. Transverse bending performance

    4.2.1. The influence of processing parameters on theflexural modulus of CF/PEEK composites

    Fig.9 presents the typical bending force-displacement curves of CF/PEEK composites specimens fabricated at different processing conditions. The CF/PEEK specimens show linear elastic characteristics until brittle failure. The different slopes of the curves reveal the variation of transverse flexural modulus (Eyy) of CF/PEEK composites with the processing parameters. With the increase of molding temperature and molding pressure,theEyyof the CF/PEEK composites increases, which is consistent with the experimental results of Zheng B et al. [23].

    The relationship between theEyyof CF/PEEK composites and the processing parameters is summarized in Fig.10. In order to more intuitively investigate the coupling effect of processing parameters on mechanical properties of CF/PEEK composites,the contour map of theEyyunder different processing parameters is obtained by interpolating the results of the orthogonal experiments,as seen in Fig.10(b)—Fig.10(d)From the experimental data in Fig.10(a),it can be found that the effect of processing parameters onEyyis not linear.According to Fig.10(b)and Fig.10(c),the increase of molding temperature reduces the viscosity of the resin, and the increase of molding pressure and holding time promotes the infiltration of fibers with resin,thus improving theEyy,and a similar trend is found in other literature [22]. Meanwhile, increasing the molding pressure can increase the density of the crystallization domain,reduce the crystal gap, and further increase the contact boundary area of crystals.Due to the high stiffness of the crystal boundary structure,which improves the modulus of the CF/PEEK composites.Similar to the results of theGICanalysis, the longer holding time at higher temperatures results in PEEK degradation and crosslinking [27],which reduces theEyy,as shown in Fig.10(d).The detailed analysis of the influence of molding process parameters on crystallization and the effect of crystallization on mechanical properties is carried out in Sections 4.3 and 4.4.

    Fig.10. Relationship between Eyy and molding process parameters of CF/PEEK composites:(a)Orthogonal test results of Eyy;(b)Contour map of molding temperature and molding pressure; (c) Contour map of molding pressure and holding time; (d) Contour map of holding time and molding temperature.

    The curves above the contour maps in Fig.10(b)—Fig.10(d) are the trend graphs of the three process parameters onEyyaccording to range analysis. The results show that the influence order of process parameters onEyyis the same asGIC,and the recommended molding process parameters are 405?C,1.5 MPa and 30 min with the objective ofEyy.

    4.2.2. The influence of molding parameters on the fracture morphology of three-point bending specimens

    To analyze the effects of the processing parameters on the failure mechanism of CF/PEEK composites, the fracture morphologies of the three-point bending specimens fabricated at different temperatures and pressures are observed using SEM. As shown in Fig. 11(a) and Fig. 11(b), exposed carbon fibers and the fibers debonding can be observed in the fracture of the specimens. This reflects that the movement of PEEK resin molecular chain segments of PEEK resin under lower molding temperature and pressure is impeded. Higher energy is required to overcome the movement between the chain segments, which is manifested by high resin viscosity and poor fluidity, resulting in incomplete penetration of the matrix, high porosity of the composites, and poor fiber/matrix interface strength. As the molding temperature and pressure increase,Fig.11(c)and Fig.11(d)show that the exposed carbon fibers and the voids are significantly reduced. These indicate that increasing the molding temperature and pressure can ensure the fiber/resin interface strength and improve resin and fiber infiltration while making the composite laminate denser and reducing porosity, thus enhancing the bending performance of the CF/PEEK composites.

    Fig.11. SEM micrographs of the three-point bending fracture surfaces of specimens fabricated at different molding process conditions: (a) 360 ?C, 0.25 MPa (40 min); (b) 375 ?C,0.5 MPa (20 min); (c) 390 ?C,1 MPa (40 min); (d) 405 ?C,1.5 MPa (20 min).

    The fracture morphologies of the three-point bending specimens fabricated at different holding times are observed in Fig.12.As shown in Fig. 12(a) and Fig. 12(b), the fiber/matrix debonding can be observed at the fracture of specimens.This is mainly due to the inability of the fibers and the matrix to fully infiltrate in a short time, which leads to a weaker bonding interface of the CF/PEEK composites. As the holding time increases, as shown in Fig.12(c)and Fig.12(d), it can be observed that the resin attached to the fibers has increased. These clarify that increasing the holding time can increase the fiber/matrix interface strength,thereby improving the transverse bending performance of the CF/PEEK composites.

    Fig.12. SEM micrographs of the three-point bending fracture surfaces of specimens fabricated at different molding process conditions: (a) 10 min (360 ?C, 0.5 MPa); (b) 20 min(390 ?C, 0.25 MPa); (c) 30 min (375 ?C,1 MPa); (d) 40 min (405 ?C, 0.5 MPa).

    Fig. 13. DSC results of CF/PEEK composites fabricated under different heating histories: (a) Heat flow-temperature curves; (b) Relationship between crystallinity, melting temperature, and molding temperature.

    4.3. The influence of processing parameters on the crystallization of CF/PEEK composites

    Generally, the decrease in crystallinity leads to a reduction in stiffness and strength of semi-crystalline polymers but an increase in ductility due to fewer secondary intermolecular bonds and an increase in disorder. Therefore, it is essential to investigate the effect of molding process parameters on the crystallization behavior of semi-crystalline polymer composites.To reveal the effects of the processing parameters on CF/PEEK composites, DSC tests are applied on the CF/PEEK specimens after thermoforming. The DSC curves are shown in Fig.13(a). The crystallinity of CF/PEEK specimens is calculated according to Eq. (2), as shown in Fig.16(a).

    As shown in Fig.13,the melting temperature decreases with the increase of molding temperature and increases with the increase of molding pressure. This is because, on the one hand, the melting temperature decreases as the molding temperature increases from 360 to 405?C, and a similar trend has been found in other studies[42]. The decrease in melting temperature may be related to the reduction of the number of remaining crystalline entities and the change in the molecular structure of the PEEK matrix.On the other hand, molten resin mobility increases with molding pressure,accompanied by increased melt shear effects leading to enhance molecular chain orientation, thereby increasing the melting temperature of the PEEK matrix. In addition, as shown in Fig.13(b), it can be seen that the crystallinity remains relatively constant as the molding temperature increase. This is also consistent with the conclusions of other studies that the molding temperature mainly affects the number and size of crystalline entities but does not change the ultimate crystallinity level of the composite material[42].

    The melting temperature of semi-crystalline polymer composites is determined by factors such as crystal size, folding surface energy and plate thickness [38]. Fig.14(a) shows the microscopic morphology of the CF/PEEK fracture fabricated at 405?C,1.5 MPa,and 20 min process parameters. It can be observed that highoriented spherulites are distributed on the fiber surface, and these spherulites constitute the columnar crystalline structure of high quality. Schematic diagram of the high-oriented spherulites generated on the fiber surface, as shown in Fig.14(b). This is also consistent with the conclusions of other studies that the lower the matrix melting temperature, the larger the size of the spherical crystal, and the higher the molecular integrity. Conversely, the higher the matrix melting temperature, the smaller the spherical crystal size[43,44].The crystal structures formed at lower molding temperatures are not well defined,mainly due to the low mobility of the polymer chains when the molding temperature is low,which limits the ability of the chains to diffuse to the growing crystal fronts.Moreover,columnar crystal structures can be observed only when the molding temperature is high enough to destroy the preexisting crystalline entities [42]. Therefore, based on the above results, it can be concluded that the higher the molding temperature,the larger size of the well-defined spherical crystals generated in the CF/PEEK composites,and the number of crystals is lower than that of the specimen fabricated at lower molding temperatures.

    Fig.14. (a) SEM observation of the columnar crystalline structures and (b) schematic diagram of high-oriented spherulites on the fiber surface.

    The relationship between molding process parameters,lamella,and fiber-matrix bonding mechanisms on the degree of crystallinity is shown in Fig.15.The micro-morphology of the fiber surface of the specimen fabricated at 405?C,0.5 MPa,and 40 min is shown in Fig.15(a).The results indicate that higher molding temperatures and longer holding time allow the PEEK matrix tends to diffuse and strongly adsorbs to the fiber surface, which is consistent with the conclusion of Brady R L et al. [45]. The schematic diagram of the fiber-matrix interaction of the CF/PEEK composites in Fig. 15 is similar to the other studies [38]. The flattened crystalline lamellar chains with high crystallinity in the interfacial region enable more polar components to interact functionally with the fiber surface.The adhesion of the interfacial region is increased,which affects the mechanical properties of the composites,such as improving shear performance. In contrast, holding for a longer time at a lower molding temperature reduces the viscosity of the molten PEEK matrix. Due to the crosslinking of PEEK, the mobility of crystallizable unit molecules is further reduced,which affects the nucleation mechanism and slows down the crystal growth. Thus, the PEEK matrix is unable to develop strong bonds with the fiber surface,as shown in Fig.15(b),which is fabricated at 360?C,0.25 MPa,40 min.

    Fig.15. SEM of fracture surface and schematic diagram of fiber-matrix interaction of CF/PEEK composites under different molding process conditions: (a) SEM fracture surface of high crystallinity specimen (XC = 32.41%); (b) SEM fracture surface of low crystallinity specimen (XC = 23.54%).

    The DSC test results of CF/PEEK composites under different processing parameters are calculated and drawn in Fig.16(a).It can be seen that the crystallinity of the CF/PEEK composites fabricated by the orthogonal process ranged from 23.5 to 33.6%.The molding temperature affects the destruction of the pre-existent crystalline entities and the formation of new nuclei, but since the molding temperature mainly affects the number and size of crystalline entities, it does not affect the final crystallinity of the CF/PEEK composites. Therefore, the degree of crystallinity remains relatively constant as the molding temperature increases, as shown in Fig.16(b).Molding pressure and holding time are as well important for the crystallization behavior of CF/PEEK composites.The molding pressure orients the polymer melt and induces nucleation, which leads to a higher crystallization rate.However,the slight difference of each molding pressure in the thermoforming process leads to an unobvious effect of the molding pressure on the crystallinity, as shown in Fig. 16(c). As the holding time increases, the chain oxidation and crosslinking of the PEEK matrix leads to a decrease in the molecular mobility of crystallizable units in the melt, which influences the nucleation mechanism and slows down the crystal growth process, as shown in Fig.16(d), and a similar trend is proposed in other literature[46].In addition,appropriately increasing the holding time can generate transverse crystals on the carbon fiber surface [42], thus increasing the stiffness of the composites,but extremely short and extremely long holding time would reduce the transverse crystals [47].

    Fig. 16. Relationship between crystallinity and molding process parameters of CF/PEEK composites: (a) Orthogonal test results of crystallinity; (b) Contour map of molding temperature and molding pressure; (c) Contour map of molding pressure and holding time; (d) Contour map of holding time and molding temperature.

    4.4. The relationship between molding process parameters,crystallization and mechanical properties

    In the above Sections, the influence mechanism of processing parameters on the mechanical properties and crystallinity of CF/PEEK composites is discussed, respectively. However, it has been reported that the crystallinity of resin has a significant effect on mechanical properties [31], clarifying the inherent relationship between process parameters, crystallization and mechanical properties can further optimize the manufacturing process of thermoplastic composites. Schematic diagrams of deformation in the crystalline and amorphous domains of the DCB and the threepoint bending specimens are shown in Fig.17 and Fig.18. Due to the macromolecular chains in the crystalline domain aligning in better order and owning stronger intermolecular forces, resulting in higher strength and rigidity [48,49], the matrix becomes more stiff and brittle after crystallization,as shown in Fig.17 and Fig.18.Thus,the higher crystallinity enhances the bending performance of CF/PEEK composites, as shown in Fig.18. However, the ductility of the matrix plays a dominant role in the crack extension of the DCB specimen. As the crystallinity increases, the percentage of ductile amorphous domains decreases, which reduces theGICof CF/PEEK composites,as shown in Fig.17.

    Fig.17. Schematic diagram of mode-I delamination of semi-crystalline CF/PEEK composites specimen.

    Fig. 18. Schematic diagram of semi-crystalline CF/PEEK composites specimen deformation under bending load: (a) Schematic drawing of the bending test; (b) Deformation of crystalline and amorphous domains under bending load.

    Fig.19. Trend graph of mechanical properties changing with crystallinity: (a) Mode-I interlaminar fracture toughness; (b) Transverse flexural modulus.

    Fig. 20. SEM micrographs of spherulitic structures of the specimen are fabricated at 405 ?C,1.5 MPa, and 20 min.

    Molding temperature has a slight effect on matrix crystallinity,but higher molding temperatures can reduce molten PEEK viscosity and improve fiber-matrix infiltration,thereby increasing theGICof CF/PEEK composite laminate.Molding pressure affects theGICof CF/PEEK composites from two aspects. On the one hand, the higher molding pressure increases the crystallinity of the matrix PEEK due to stress induction. The higher crystallinity means a higher percentage of brittleness in the material, while the ductility of the matrix plays a dominant role in the crack extension of the DCB specimen.On the other hand,increasing the molding pressure can effectively improve the infiltration of high-viscosity resin with fibers and lead to a denser laminate, thus improving theGIC.Therefore, for theGICof CF/PEEK composite laminate, there has a competitive relationship between the crystallinity and the molding quality (infiltration, porosity, etc.). According to the data of DCB range analysis results (Fig. 6),GICincreases with the increase of molding pressure, which means that high-quality laminates fabricated under higher molding pressure contribute more to theGICof CF/PEEK composites. The crystallinity decreases with increasing holding time, therefore a longer holding time is beneficial to improve the matrix ductility and thus theGICof CF/PEEK composites, which is consistent with the range analysis results(Fig. 6) of the DCB test data.

    The effect of molding temperature onEyyof CF/PEEK composites is similar to that ofGIC,whereEyyincreases with increasing molding temperature. It is worth noting that it is easier to generate welldefined spherulites and columnar crystalline structures at higher molding temperatures,resulting in increasedEyy. Due to the effect of stress-induced crystallization, increasing the molding pressure not only improves the crystallinity but also improves the molding quality, thus improvingEyy. The holding time affects theEyyof CF/PEEK composite laminate from two aspects. On the one hand,increasing the holding time reduces the crystallinity, which is not conducive to improvingEyy.On the other hand,although the proper increase of holding time can improve the molding quality, due to the degradation and crosslinking of resin at higher temperatures,which makes too long holding time is not conducive to the molding quality. The above conclusions are consistent with the range analysis results (Fig.10) of the three-point bending test data.

    The relationship between the mechanical properties and crystallinity of CF/PEEK composites under orthogonal processing conditions fabricated is exhibited in Fig. 19. It can be seen that the crystallinity of the PEEK matrix has an approximately linear effect on the mechanical properties.TheGICis negatively correlated with the matrix crystallinity, and conversely, theEyyis positively correlated with the matrix crystallinity. Therefore, the thermoforming process affects the mechanical properties of the composites by influencing the matrix crystallization.In addition,it is worth noting that the crystallinity of some specimens does not match their mechanical performance, mainly due to defects caused by processing parameters, as marked in Fig. 19. Indeed, the mechanical properties of composites can be affected by other factors (such as void defects), which need to be further investigated in future studies.

    The elucidation of the inherent relationship between molding process parameters, mechanical properties, and crystallization is essential for the high-quality molding of CF/PEEK composites. The studies in Sections 4.1 and 4.2 show that theGICand bending performance of CF/PEEK composites are positively correlated with the molding temperature,pressure and holding time,mainly due to the degree of fiber/matrix infiltration promoted by increasing these process parameters.However,the effect of matrix crystallization on the mechanical properties cannot be ignored.Although the study in Section 4.3 shows that the effect of molding process parameters on the crystallinity of the PEEK matrix is not highly significant, but it seriously affects the crystalline morphology,which is related to the mechanical properties of CF/PEEK composites.On the one hand,the consolidation of CF/PEEK composites should be carried out at a sufficiently high temperature to destroy the pre-existing crystalline entities in the composite prepreg,thus improving the toughness of the PEEK matrix and theGICof the CF/PEEK composites[47].On the other hand, the presence of columnar crystalline structures and spherulites improves the modulus of the composites. Although PEEK resin degrades at higher temperatures, the degradation does not prevent the formation of well-defined crystalline structures,and the crystallization domain grows with the appropriate increase in holding time [42,47], thus increasing theEyyof composites. As observed for the spherulitic structures of CF/PEEK composites fabricated at 405?C,1.5 MPa and 20 min in Fig.20.In addition,the increased molding pressure not only promotes the penetration of the resin into the fiber, but also increases the density of the crystalline domain and reduces the crystal gap. Due to the stressinduced nucleation, the crystallization rate is accelerated, thereby increasing the crystallinity and the mechanical properties of the composites. Therefore, the influence of the molding process on crystallization behavior significantly affects the mechanical properties of CF/PEEK composites.

    5. Conclusions

    In order to improve the molding quality of thermoplastic composites for extension and application in the cutting-edge equipment of the aerospace and defence fields, the process/crystallization/property inherent relationships of continuous CF/PEEK composites were studied in this work.The CF/PEEK composite laminates were fabricated via thermoforming, using the threeparameter four-level orthogonal test. The performance of CF/PEEK composite laminates was analyzed by mechanical characterization,crystallization characterization, and microscopic observations.The main conclusions are as follows:

    (1) The mode-I interlaminar fracture toughness and transverse flexural modulus are positively related to the molding temperature, pressure and holding time. The mechanical properties of CF/PEEK composites are not only affected by the degree of matrix/fiber infiltration and molding quality, but also by potential matrix crystallization. The increased molding temperature, pressure and holding time can improve the degree of fiber/matrix infiltration and reduce molding defects such as voids, which improves mechanical properties. However, it is necessary to note that long-time high-temperature conditions can alter the viscosity and properties of the matrix due to crosslinking and degradation,thereby reducing the molding quality.

    (2) The molding process parameters affect the crystallinity and crystalline morphology of the matrix, which in turn affects the mechanical properties of the composites. The results show that the crystallinity of the matrix has an almost linear influence on the mechanical properties of CF/PEEK composites. Sufficiently high molding temperature can improve the toughness and mode-I interlaminar fracture toughness of the composites by destroying pre-existing crystallites.Although increasing the holding time affects the nucleation mechanism and decreases the crystallinity due to matrix degradation, it can form well-defined crystalline structures,which increases the flexural modulus of the composites.Increased molding pressure can increase the crystallization rate due to stress-induced nucleation,and it can increase the density of the crystallization domain, which improves the mechanical properties of the composites.

    (3) The above results suggest that the optimal process parameter array in certain process conditions are molding temperature of 405?C,molding pressure of 1.5 MPa,and holding time of at least 30 min based on the thermoforming method. This processing condition ensures excellent transverse bending performance and mode-I interlaminar fracture toughness of the continuous CF/PEEK composites.

    Data availability statement

    Research data are not shared.

    Declaration of competing interest

    The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

    Acknowledgements

    The authors of this paper acknowledge the financial support of the National Natural Science Foundation of China (NO. 11902255,U1837601 and 52090051).

    Appendix A. Supplementary data

    Supplementary data to this article can be found online at https://doi.org/10.1016/j.dt.2022.04.010.

    女警被强在线播放| 99精品在免费线老司机午夜| 久热爱精品视频在线9| 久久婷婷成人综合色麻豆| 91成人精品电影| 亚洲男人天堂网一区| 国产成人精品无人区| 久久久精品国产亚洲av高清涩受| 精品国内亚洲2022精品成人| 一级a爱视频在线免费观看| 欧美av亚洲av综合av国产av| 91成年电影在线观看| 欧美成狂野欧美在线观看| 国产亚洲欧美精品永久| netflix在线观看网站| 亚洲国产高清在线一区二区三 | 丝袜美腿诱惑在线| 在线av久久热| 一级毛片高清免费大全| 亚洲av成人不卡在线观看播放网| 亚洲av电影在线进入| av福利片在线| 久久久久久久久中文| 成人av一区二区三区在线看| 啦啦啦 在线观看视频| 午夜福利视频1000在线观看| 午夜免费鲁丝| 亚洲一区二区三区色噜噜| 国产欧美日韩一区二区三| 色播亚洲综合网| 婷婷丁香在线五月| 精品福利观看| 久久精品国产清高在天天线| 午夜精品在线福利| 日日爽夜夜爽网站| 国产av在哪里看| 91成年电影在线观看| 一进一出抽搐动态| 一本综合久久免费| 国产一区在线观看成人免费| 老鸭窝网址在线观看| 人妻久久中文字幕网| 国产成+人综合+亚洲专区| 国产男靠女视频免费网站| 90打野战视频偷拍视频| 欧美乱妇无乱码| 日本三级黄在线观看| 99精品在免费线老司机午夜| 女人爽到高潮嗷嗷叫在线视频| 国产精品免费视频内射| 美女国产高潮福利片在线看| 国产男靠女视频免费网站| 91麻豆精品激情在线观看国产| or卡值多少钱| 精品熟女少妇八av免费久了| 亚洲精品国产一区二区精华液| 成人欧美大片| 精品国产超薄肉色丝袜足j| 巨乳人妻的诱惑在线观看| 天堂动漫精品| 欧美成人一区二区免费高清观看 | 久久国产乱子伦精品免费另类| 久久精品国产亚洲av香蕉五月| 久久久久久大精品| 久9热在线精品视频| 午夜久久久在线观看| 亚洲 欧美一区二区三区| 天天一区二区日本电影三级| 亚洲精品在线观看二区| 欧美黄色片欧美黄色片| а√天堂www在线а√下载| a在线观看视频网站| 热99re8久久精品国产| 精品久久久久久久末码| 久久精品国产99精品国产亚洲性色| 久久久久久久久免费视频了| 欧美激情久久久久久爽电影| 在线观看一区二区三区| 国产精品精品国产色婷婷| 麻豆av在线久日| 国产国语露脸激情在线看| svipshipincom国产片| 欧美大码av| 91九色精品人成在线观看| 黄网站色视频无遮挡免费观看| 欧美av亚洲av综合av国产av| 欧美性猛交黑人性爽| 午夜老司机福利片| 观看免费一级毛片| 黑人巨大精品欧美一区二区mp4| 精品久久久久久,| 免费高清视频大片| 青草久久国产| 制服人妻中文乱码| 久热爱精品视频在线9| 日韩欧美国产一区二区入口| 18禁国产床啪视频网站| 国产高清有码在线观看视频 | 成人国产一区最新在线观看| 欧美日韩亚洲综合一区二区三区_| 高清毛片免费观看视频网站| 久久国产精品人妻蜜桃| 少妇粗大呻吟视频| 99在线人妻在线中文字幕| 日本 欧美在线| 桃色一区二区三区在线观看| 看片在线看免费视频| 精品高清国产在线一区| 国产一级毛片七仙女欲春2 | 亚洲在线自拍视频| 免费无遮挡裸体视频| 此物有八面人人有两片| 中文字幕人妻丝袜一区二区| 色精品久久人妻99蜜桃| 亚洲第一欧美日韩一区二区三区| 窝窝影院91人妻| 亚洲三区欧美一区| 久久精品国产清高在天天线| 色精品久久人妻99蜜桃| 欧美中文综合在线视频| 白带黄色成豆腐渣| 亚洲国产欧美日韩在线播放| 嫩草影院精品99| 在线观看日韩欧美| 制服人妻中文乱码| 国产视频一区二区在线看| 国产精品香港三级国产av潘金莲| 嫩草影院精品99| 欧美日韩福利视频一区二区| 高潮久久久久久久久久久不卡| 欧美精品亚洲一区二区| 亚洲精品久久成人aⅴ小说| 午夜亚洲福利在线播放| 成人亚洲精品av一区二区| 国产精品亚洲美女久久久| 日韩 欧美 亚洲 中文字幕| 久久人妻福利社区极品人妻图片| av福利片在线| 成年版毛片免费区| 免费av毛片视频| 91av网站免费观看| 欧美另类亚洲清纯唯美| 免费无遮挡裸体视频| 亚洲第一av免费看| 禁无遮挡网站| 91老司机精品| 黄色 视频免费看| 国产一区二区三区在线臀色熟女| 亚洲精华国产精华精| www国产在线视频色| 国产乱人伦免费视频| 国产又爽黄色视频| 国产成人精品无人区| 国产人伦9x9x在线观看| 国产精品1区2区在线观看.| 亚洲国产精品sss在线观看| 亚洲av日韩精品久久久久久密| 国产成人av教育| 黄片播放在线免费| 夜夜看夜夜爽夜夜摸| 欧美日韩中文字幕国产精品一区二区三区| 青草久久国产| 高潮久久久久久久久久久不卡| 中文亚洲av片在线观看爽| 一区二区日韩欧美中文字幕| 中亚洲国语对白在线视频| 特大巨黑吊av在线直播 | 久久久精品欧美日韩精品| 欧美成狂野欧美在线观看| 精品第一国产精品| 夜夜看夜夜爽夜夜摸| 亚洲成人国产一区在线观看| 给我免费播放毛片高清在线观看| 一级毛片女人18水好多| 老汉色∧v一级毛片| 草草在线视频免费看| 亚洲精品中文字幕一二三四区| 国产日本99.免费观看| 丁香六月欧美| 久久久久久免费高清国产稀缺| 一进一出好大好爽视频| 丝袜人妻中文字幕| 九色国产91popny在线| 亚洲人成网站在线播放欧美日韩| 亚洲国产欧洲综合997久久, | 老熟妇仑乱视频hdxx| 国产欧美日韩一区二区三| av超薄肉色丝袜交足视频| 欧美中文日本在线观看视频| 韩国av一区二区三区四区| 天天躁夜夜躁狠狠躁躁| 淫秽高清视频在线观看| 一进一出抽搐动态| 一本综合久久免费| 久久精品aⅴ一区二区三区四区| av福利片在线| 国产伦一二天堂av在线观看| 人人妻,人人澡人人爽秒播| 国产精品九九99| 国产av又大| 高潮久久久久久久久久久不卡| 两个人免费观看高清视频| 黑丝袜美女国产一区| 欧美丝袜亚洲另类 | 色精品久久人妻99蜜桃| √禁漫天堂资源中文www| 精品高清国产在线一区| 欧美黑人精品巨大| 青草久久国产| 波多野结衣巨乳人妻| 日本免费一区二区三区高清不卡| 亚洲久久久国产精品| 亚洲av熟女| 亚洲avbb在线观看| 国产成+人综合+亚洲专区| 一级a爱片免费观看的视频| 搡老妇女老女人老熟妇| 午夜成年电影在线免费观看| 一级a爱视频在线免费观看| 久久天堂一区二区三区四区| 51午夜福利影视在线观看| 欧美人与性动交α欧美精品济南到| 搞女人的毛片| 午夜a级毛片| 视频在线观看一区二区三区| 亚洲国产精品久久男人天堂| www.自偷自拍.com| 午夜免费激情av| 高潮久久久久久久久久久不卡| 999久久久精品免费观看国产| 欧美日韩中文字幕国产精品一区二区三区| 精品久久蜜臀av无| 成年版毛片免费区| 国产伦人伦偷精品视频| 国产精品永久免费网站| 精品少妇一区二区三区视频日本电影| 亚洲性夜色夜夜综合| 亚洲成国产人片在线观看| 亚洲av成人一区二区三| 亚洲精品久久成人aⅴ小说| 午夜福利在线观看吧| 国产精品 欧美亚洲| 女人高潮潮喷娇喘18禁视频| 色播亚洲综合网| 法律面前人人平等表现在哪些方面| 日韩精品青青久久久久久| 免费观看人在逋| 国产v大片淫在线免费观看| 亚洲国产欧美日韩在线播放| 黄频高清免费视频| www.熟女人妻精品国产| 日韩成人在线观看一区二区三区| 日韩大码丰满熟妇| 色综合婷婷激情| 午夜a级毛片| 国产成人影院久久av| 成人亚洲精品av一区二区| 麻豆成人av在线观看| 88av欧美| 精品熟女少妇八av免费久了| 一级黄色大片毛片| 岛国视频午夜一区免费看| 久久精品成人免费网站| 国产伦一二天堂av在线观看| 宅男免费午夜| 欧美日韩中文字幕国产精品一区二区三区| 国产在线精品亚洲第一网站| av中文乱码字幕在线| 美女高潮到喷水免费观看| 日韩一卡2卡3卡4卡2021年| www日本在线高清视频| 日本成人三级电影网站| 免费av毛片视频| 国产熟女午夜一区二区三区| 精品卡一卡二卡四卡免费| 人人妻,人人澡人人爽秒播| 午夜福利在线在线| 国内揄拍国产精品人妻在线 | 欧美日韩福利视频一区二区| 亚洲 欧美一区二区三区| 亚洲真实伦在线观看| 亚洲国产精品成人综合色| 午夜日韩欧美国产| 国产av一区二区精品久久| 国产色视频综合| 搞女人的毛片| 国产精品二区激情视频| 免费看日本二区| 亚洲专区中文字幕在线| 老鸭窝网址在线观看| 中文资源天堂在线| 国产成年人精品一区二区| 可以在线观看的亚洲视频| 中文资源天堂在线| 999久久久精品免费观看国产| 精品免费久久久久久久清纯| 人妻丰满熟妇av一区二区三区| av欧美777| 日本 欧美在线| 一级毛片女人18水好多| 88av欧美| 欧美色欧美亚洲另类二区| 国产精品野战在线观看| 国产欧美日韩精品亚洲av| 成人手机av| 久久久久免费精品人妻一区二区 | 亚洲av中文字字幕乱码综合 | 村上凉子中文字幕在线| cao死你这个sao货| 十分钟在线观看高清视频www| 午夜久久久在线观看| 亚洲精品av麻豆狂野| 亚洲av五月六月丁香网| 自线自在国产av| 黄网站色视频无遮挡免费观看| 日本 av在线| 亚洲av电影在线进入| 欧美色欧美亚洲另类二区| 色综合婷婷激情| 老鸭窝网址在线观看| 美女免费视频网站| 亚洲最大成人中文| 在线观看免费午夜福利视频| 黄色视频不卡| 亚洲熟妇中文字幕五十中出| 午夜视频精品福利| 免费在线观看亚洲国产| 在线观看免费午夜福利视频| 国产成人影院久久av| 国产精品一区二区三区四区久久 | 中文字幕高清在线视频| 亚洲天堂国产精品一区在线| 看免费av毛片| 久久热在线av| 看免费av毛片| 最近最新中文字幕大全电影3 | 亚洲av美国av| 亚洲 欧美 日韩 在线 免费| 看黄色毛片网站| 精品一区二区三区四区五区乱码| 色精品久久人妻99蜜桃| 男女床上黄色一级片免费看| 黄频高清免费视频| 亚洲九九香蕉| 级片在线观看| 亚洲专区中文字幕在线| 亚洲精品中文字幕一二三四区| 人妻丰满熟妇av一区二区三区| 日本五十路高清| 亚洲五月天丁香| 成人欧美大片| 国产免费av片在线观看野外av| 国产成人一区二区三区免费视频网站| 精品久久久久久久久久久久久 | 午夜激情福利司机影院| √禁漫天堂资源中文www| 一级片免费观看大全| 人人妻人人澡欧美一区二区| 日韩成人在线观看一区二区三区| 一二三四社区在线视频社区8| 中文字幕人成人乱码亚洲影| 久久婷婷人人爽人人干人人爱| 亚洲激情在线av| 90打野战视频偷拍视频| 亚洲精品美女久久av网站| 婷婷六月久久综合丁香| 亚洲中文字幕日韩| 每晚都被弄得嗷嗷叫到高潮| 午夜日韩欧美国产| 国产精品野战在线观看| 无限看片的www在线观看| 成年免费大片在线观看| 国产精品永久免费网站| 神马国产精品三级电影在线观看 | 男女床上黄色一级片免费看| 99久久综合精品五月天人人| 一进一出抽搐gif免费好疼| 久久午夜亚洲精品久久| 欧美日韩瑟瑟在线播放| АⅤ资源中文在线天堂| 日日爽夜夜爽网站| 听说在线观看完整版免费高清| 午夜福利成人在线免费观看| 一级黄色大片毛片| 高清毛片免费观看视频网站| 欧美乱色亚洲激情| 美女高潮喷水抽搐中文字幕| 精品久久久久久久久久免费视频| 99re在线观看精品视频| 久久久久九九精品影院| 日韩大尺度精品在线看网址| 1024香蕉在线观看| 特大巨黑吊av在线直播 | 午夜福利视频1000在线观看| 亚洲国产高清在线一区二区三 | 人成视频在线观看免费观看| 观看免费一级毛片| 欧美午夜高清在线| 三级毛片av免费| 亚洲真实伦在线观看| 香蕉国产在线看| 国产亚洲精品一区二区www| 免费女性裸体啪啪无遮挡网站| 亚洲精品av麻豆狂野| av有码第一页| 脱女人内裤的视频| 丰满的人妻完整版| 久久国产精品人妻蜜桃| 午夜福利欧美成人| 国产成人av教育| 国产亚洲精品av在线| 免费电影在线观看免费观看| 国产成人欧美在线观看| 久久99热这里只有精品18| 亚洲人成电影免费在线| 婷婷精品国产亚洲av在线| 99精品久久久久人妻精品| 色婷婷久久久亚洲欧美| 一级片免费观看大全| 国产成+人综合+亚洲专区| 亚洲av日韩精品久久久久久密| 成人18禁高潮啪啪吃奶动态图| 婷婷六月久久综合丁香| 国产亚洲欧美精品永久| 婷婷六月久久综合丁香| 成熟少妇高潮喷水视频| 女同久久另类99精品国产91| 1024手机看黄色片| 两性午夜刺激爽爽歪歪视频在线观看 | 听说在线观看完整版免费高清| 国产亚洲精品一区二区www| 黄色视频不卡| 欧美日韩亚洲国产一区二区在线观看| 精品国产美女av久久久久小说| 夜夜夜夜夜久久久久| 人人妻,人人澡人人爽秒播| 一级作爱视频免费观看| 日韩中文字幕欧美一区二区| 亚洲色图 男人天堂 中文字幕| 日日摸夜夜添夜夜添小说| 亚洲国产精品sss在线观看| 99在线视频只有这里精品首页| 久久精品国产99精品国产亚洲性色| 亚洲精品久久成人aⅴ小说| 中文字幕精品亚洲无线码一区 | 亚洲一区二区三区不卡视频| ponron亚洲| 日本免费a在线| 成人午夜高清在线视频 | 又黄又爽又免费观看的视频| 精品国产国语对白av| 91成人精品电影| 日本a在线网址| 午夜免费激情av| 最近最新中文字幕大全电影3 | 国产熟女xx| 婷婷六月久久综合丁香| 国产av又大| 国产精品亚洲美女久久久| 亚洲精品粉嫩美女一区| 制服诱惑二区| 99国产精品99久久久久| 成人国产一区最新在线观看| 午夜亚洲福利在线播放| 午夜成年电影在线免费观看| 波多野结衣av一区二区av| 又大又爽又粗| 精品久久久久久久久久免费视频| 波多野结衣高清无吗| 久久人妻福利社区极品人妻图片| 亚洲av中文字字幕乱码综合 | 亚洲精品色激情综合| 久99久视频精品免费| 搞女人的毛片| 一二三四社区在线视频社区8| 别揉我奶头~嗯~啊~动态视频| 熟妇人妻久久中文字幕3abv| 欧美日本亚洲视频在线播放| 免费高清视频大片| 精品无人区乱码1区二区| 欧美绝顶高潮抽搐喷水| 国产主播在线观看一区二区| 久久久久久人人人人人| 精品久久久久久,| 久久精品成人免费网站| 脱女人内裤的视频| 在线观看www视频免费| 久久久水蜜桃国产精品网| www.精华液| 亚洲午夜精品一区,二区,三区| 他把我摸到了高潮在线观看| 精品久久久久久久末码| 精品久久久久久久久久免费视频| 国产爱豆传媒在线观看 | e午夜精品久久久久久久| 啦啦啦韩国在线观看视频| 自线自在国产av| 亚洲狠狠婷婷综合久久图片| 99久久综合精品五月天人人| 婷婷精品国产亚洲av| ponron亚洲| 日本免费a在线| 欧美久久黑人一区二区| 国产精品影院久久| 精品久久久久久久末码| 一级毛片精品| 成年版毛片免费区| 国产精品免费一区二区三区在线| 黄色视频不卡| 亚洲av日韩精品久久久久久密| 人妻久久中文字幕网| 色哟哟哟哟哟哟| 亚洲av日韩精品久久久久久密| 精品日产1卡2卡| 免费在线观看影片大全网站| 1024视频免费在线观看| 一级黄色大片毛片| 在线观看午夜福利视频| 欧美绝顶高潮抽搐喷水| av在线天堂中文字幕| 国产成人av激情在线播放| 99精品欧美一区二区三区四区| 制服人妻中文乱码| 岛国视频午夜一区免费看| 午夜成年电影在线免费观看| 91麻豆精品激情在线观看国产| 桃色一区二区三区在线观看| 欧美激情 高清一区二区三区| 高清在线国产一区| 在线免费观看的www视频| 欧美丝袜亚洲另类 | 黑人欧美特级aaaaaa片| 黄色 视频免费看| 又大又爽又粗| 黑人操中国人逼视频| 色综合亚洲欧美另类图片| 国产av一区在线观看免费| 一级毛片女人18水好多| 亚洲成av人片免费观看| 久久久久久人人人人人| 精品一区二区三区四区五区乱码| 欧美一区二区精品小视频在线| 一区二区日韩欧美中文字幕| 欧美色欧美亚洲另类二区| 黄色丝袜av网址大全| 亚洲精品国产区一区二| 国产精品自产拍在线观看55亚洲| www.熟女人妻精品国产| 国产伦一二天堂av在线观看| 日本 av在线| 午夜精品久久久久久毛片777| 久久精品国产综合久久久| 久久狼人影院| 51午夜福利影视在线观看| 婷婷亚洲欧美| or卡值多少钱| 一本精品99久久精品77| 成人精品一区二区免费| 国产免费av片在线观看野外av| 欧美不卡视频在线免费观看 | 黄片小视频在线播放| 老司机午夜十八禁免费视频| 手机成人av网站| 日韩欧美三级三区| 人人妻人人澡人人看| 欧美精品亚洲一区二区| 亚洲国产精品合色在线| 国产精品久久久久久亚洲av鲁大| 亚洲一卡2卡3卡4卡5卡精品中文| 亚洲一区二区三区色噜噜| 免费在线观看黄色视频的| 国产精品亚洲一级av第二区| 极品教师在线免费播放| 怎么达到女性高潮| av欧美777| 久久亚洲真实| 免费在线观看成人毛片| 黑人操中国人逼视频| 欧美不卡视频在线免费观看 | 日韩大码丰满熟妇| 两性午夜刺激爽爽歪歪视频在线观看 | 女人爽到高潮嗷嗷叫在线视频| 久久精品国产清高在天天线| 国产日本99.免费观看| 亚洲专区国产一区二区| or卡值多少钱| 黑人欧美特级aaaaaa片| 国产高清视频在线播放一区| 国产精品久久久久久人妻精品电影| 成人欧美大片| 亚洲成人国产一区在线观看| 听说在线观看完整版免费高清| 国产又黄又爽又无遮挡在线| 97碰自拍视频| 精品欧美国产一区二区三| 黄色成人免费大全| 91av网站免费观看| 国产1区2区3区精品| 国产精品二区激情视频| 中文字幕人妻熟女乱码| 亚洲色图av天堂| 日本免费a在线| 国内精品久久久久精免费| 两个人免费观看高清视频| 非洲黑人性xxxx精品又粗又长| 久久精品国产综合久久久| 免费看a级黄色片| 少妇裸体淫交视频免费看高清 | 精品久久久久久久久久免费视频| 国产爱豆传媒在线观看 | 国产熟女xx| 国产精品二区激情视频| 欧美另类亚洲清纯唯美| 色婷婷久久久亚洲欧美| a级毛片a级免费在线|