    Fabrication of a model specimen for understanding micro-galvanic corrosion at the boundary of α-Mg and β-Mg17Al12

    2023-03-24 09:24:14ZhengShaoMasashiNishimotoIzumiMutoYuSugawara
    Journal of Magnesium and Alloys 2023年1期

    Zheng Shao,Masashi Nishimoto,Izumi Muto,Yu Sugawara

    Department of Materials Science,Graduate School of Engineering,Tohoku University,6-6-02 Aza-Aoba,Aramaki,Aoba-ku,Sendai 980-0579,Japan

    Abstract A model specimen with a single boundary of the α/β phase simulating Mg-Al alloys was successfully fabricated by spark plasma sintering.A small electrode area of α phase or β phase was prepared using the model specimen,and the OCPs (open-circuit potentials) of each phase and a small electrode area containing the α/β phase boundary in 0.1 M NaCl at pH 8.0 were compared: the β phase exhibited a higher potential,and the α phase showed a lower potential.The OCP of the small area containing the α/β phase boundary was the intermediate value of these phases.In a small area containing α/β phase boundary,discoloration and gas bubbles were observed on the α phase,but no bubble generation was detected on the β phase.The gas bubbles were initially generated on the α phase near the β phase,but as the discoloration (corrosion) of the α phase approached the β phase,the bubbles were generated on the β phase.In micro-galvanic corrosion of the α and β phases,the β phase did not always function as the preferred cathode.The α phase partially corroded (or discolored) and became the anodes,so that the surrounding areas were most likely to be the cathodes.When corroded areas (anodes) in the α phase approached the β phase,the β phase would become cathodes.In addition to the micro-galvanic corrosion mechanism,the role of Al in corrosion resistance at the α/β phase boundary was determined by surface analysis.

    Keywords: Magnesium alloy; α/β phase boundary;Micro-scale observation technique;Micro-galvanic corrosion;Spark plasma sintering.

    1.Introduction

    Mg alloys,such as AZ91 (Mg-9mass%Al-1mass%Zn),are lightweight materials with excellent mechanical properties[1,2].The applications of Mg alloys in automobiles could significantl contribute to reducing carbon dioxide emissions[1,3].Mg alloys are fully recyclable and abundantly available,which increases their desirability in light of rising environmental consciousness [4–8].Nonetheless,the low corrosion resistance of Mg alloys [9–11] is one of the major limitations to further applications.

    Surface treatments are effective for enhancing the corrosion resistance of Mg alloys [12–15],and promising methods have been found for practical use [16–18].However,since the underlying metal may be exposed at cut edges and defects may exist,research is also being conducted on alloying elements,heat treatment,and metallurgy to improve corrosion resistance [19–22].It is well known that theβphase(Mg17Al12) is distributed intragranularly and intergranularly in Mg-Al alloys and has a significan impact on corrosion resistance [23,24].The electrode potential of theβphase is more noble than that of theαphase (Mg matrix),and it has been proposed thatβphases serve as cathodic reaction sites on Mg alloys under natural immersion conditions of chloride solutions [25–28].In addition,it is proposed that theβphase has a higher corrosion resistance than theαphase;thus,theβphase inhibits the growth of localized corrosion such as filifor corrosion [29–32].For instance,the corrosion attack progressed in theαphase and ceased when it reached theβphase [29].In addition,the corrosion resistance improves after artificially-agin heat treatment that precipitates theβphases [32].In our previous research,we observed the corrosion behavior of AZ91D Mg alloyin situand discovered that filifor corrosion was initiated and extended alongα/βlamellar structures,butβphases remained intact after filifor corrosion [33].As described previously,theβphase is regarded as advantageous for the corrosion resistance of Mg-Al alloys.Improving corrosion resistance by controllingβphase morphology is an intriguing area of study,and elucidating the electrochemical properties of theβphase is essential for achieving this objective.

    In corrosive solutions,micro-galvanic cells between theβphase and Mg-matrix (αphase) are likely to form on the surface of Mg alloys [32].To comprehend the role of theβphase in the corrosion resistance,it is desirable to measure the galvanic current;however,the current between theβandαphases cannot be measured directly on actual Mg alloys.The size ofβphase in actual Mg alloys is on the order of micrometers,and theαandβphases are in contact with each other;consequently,a conventional method of measuring the galvanic current between two separated specimens ofαphase andβphase is too far from reality.In this study,specimens with a single boundary betweenαandβphases were fabricated using spark plasma sintering (SPS),and their corrosion behavior was observedin situin 0.1 M NaCl solution.

    SPS is an innovative consolidation technology [34–36] developed in recent years.High-quality and low-porosity sintered specimens can be efficientl fabricated by passing a pulsed electric current directly through the powder in a die while applying pressure[36–47].SPS has also been utilized in the fabrication of Mg alloys,and research on enhancing the strength and other mechanical properties of Mg alloys has been published [41–43].However,there are only a handful of studies on the corrosion-resistant Mg alloys fabricated by SPS [44–46].Moreover,to our knowledge,SPS has not been used to fabricate specimens simulating the boundary between theαandβphases in Mg-Al alloys.

    This study aims to fabricate a model specimen simulating theα/βphase boundary of Mg-Al alloy and to elucidate the micro-galvanic action at the boundary in a chloride solution.In this study,starting raw materials for SPS were chosen,and the effects of sintering conditions of holding temperature and time on the formation of the boundary betweenαandβphases were analyzed.The micro-galvanic corrosion behavior betweenαandβphases was observedin situin 0.1 M NaCl solution.Comparatively,corrosion behavior was also observed on electrode composed of onlyαphase or onlyβphase.

    2.Materials and methods

    2.1.Spark plasma sintering (SPS)

    Fig.1.(a) Schematic illustration of the SPS device and (b) layer pattern of the starting raw materials fille in a graphite die.

    SPS was used to fabricate model specimens with a singleα/βphase boundary of a Mg-Al alloy.Fig.1 shows a schematic illustration of the SPS device and the layer pattern of the starting raw materials in a graphite die (diameter:15 mm).Pure Mg sheet (purity: 99.9%,thickness: 0.25 mm),pure Mg powder (purity: 99.5%,particle size: 180 μm),pure Al sheet (purity: 99%,thickness: 5 mm),pure Al foil (purity: 99.999%,thickness: 0.10 mm),pure Al powder (purity:99.9%,particle size: 106–180 μm),and pure Al powder (purity: 99.99%,particle size: 45 μm) were used.These starting raw materials were fille into the SPS die as the following scheme in a glove box under Ar atmosphere,and anα/βphase boundary was intended to fabricate between Layers 2 and 3 and between Layers 3 and 4.To prevent the leakage of Mg-melt from the die during sintering,0.84 g of pure Al powders (purity: 99.9%,particle size: 106–180 μm,height in the die:ca.1.75 mm) were fille as Layer 1,followed by an Mg sheet or 0.23 g of Mg powders (height in the die:ca.0.75 mm).As Layer 3,an Al sheet or Al powder was then applied.Subsequently,the same materials as Layer 2 were used to create Layer 4,and then 0.84 g of 99.9% pure Al powder was used to create Layer 5.To obtain fla boundaries between each layer,each time after fillin Layers 2,3,and 5,a 2–3 kN pressure was applied under an Ar atmosphere.

    A pulsed current was applied to the starting raw materials(SPS specimen) in the graphite die under 30 MPa of pressure in an Ar atmosphere during the sintering process.Unless otherwise specified the heating rate was 25 °C min?1and the holding temperature was 420 °C.Moreover,the holding time were changed from 30 min to 120 min.The SPS specimen was cooled to room temperature in an Ar-fille chamber following sintering.Additionally,the cylindrical SPS specimen with a height ofca.5 mm and a diameter of 15 mm was then cut vertically into two equal pieces,and the cross-sections were utilized in experiments.The cross-section was mechanically ground with SiC paper through a 1500 grit,and then finishe with 1 μm diamond paste.Finally,the specimens were rinsed with ethanol and dried with a gentle blow of N2gas.

    2.2.Materials characterization

    The specimens were etched in a mixture of 1.5 mL HNO3and 80 mL ethanol forca.2 s at 25 °C,and the microstructures were observed using an optical microscope and a field-emissio scanning electron microscope(FE-SEM).Additionally,energy-dispersive X-ray spectroscopy (EDS)was conducted to analyze chemical compositions.During SEM observation and EDS analysis,the vacuum level was 5.4×10?5Pa and accelerating voltage was 20 kV.The etched surfaces of the specimens were also analyzed using an electron probe micro analyzer (EPMA).The voltage for acceleration was set to 15 kV.The cross-sections of the specimens were fabricated by a Ga+focused ion beam and observed with scanning transmission electron microscope(STEM).Additionally,electron diffraction was performed to identify crystal structures.The X-ray diffraction (XRD) patterns were obtained using Cu Kαradiation and the diffraction patterns were collected over a 2θrange of 20–90° with a step width of 0.02°.A scan rate of 2° min?1was maintained and the contribution of Cu Kα2 was eliminated using computer software.

    2.3.Open-circuit potential (OCP) measurements

    The OCP measurements were conducted in a naturally aerated 0.1 M NaCl solution at 25 °C.The pH of the solution was adjusted to 8.0 with NaOH.A battery-powered potentiostat [47] and anin situreal-time observation system similar to that developed by Chiba et al.,[48] were used.The immersion periods were 10 and 60 min.The specimen surfaces were masked with a silicone sealant,with the exception of the working electrode area,and the sealant was cured for 12 h at 25°C andca.50%relative humidity.The size of the electrode area wasca.600 μm×ca.700 μm for the OCP measurements of the electrode with anα/βphase boundary.The electrode area wasca.660 μm ×ca.1000 μm used for the measurements of theαphase.In the case ofβphase measurements,the size of the electrode area wasca.100 μm ×ca.150 μm.The electrode potentials were measured using an Ag/AgCl(3.33 M KCl) electrode.The electrode potentials in this paper are givenversusthe Ag/AgCl (3.33 M KCl).The surface appearance of the working electrode was recorded as a movie using a CCD (charge-coupled device) camera attached to an optical microscope,and the movie was saved in the MP4 format.After the experiment was completed,time-lapse images (TIFF format) were made from the movie.

    2.4.Surface analysis

    Auger electron spectroscopy (AES) was performed to obtain the depth profil of the chemical compositions on the specimen surfaces.The analyzed areas were approximately 400 μm2.The voltage of the electron beam was 5 kV,and the beam current was 5 nA.Moreover,sputtering was performed with Ar+at an accelerating voltage of 2 kV with a 30° tilt.The depth was computed based on the sputtering rate of SiO2(1.13 nm min?1).

    3.Results and discussion

    3.1.Fabrication of α/β phase boundary by SPS

    3.1.1.Feasibility assessment

    In the firs attempt,instead of the layer pattern shown in Fig.1,an Mg sheet(thickness:0.25 mm,diameter:ca.10 mm)surrounded by Al powder (purity: 99.9%,particle size: 106–180 μm) was used for the SPS.Since the eutectic reaction in the Mg-Al phase diagrams occurs at approximately 437 °C[49],the sintering was conducted for 30 min at 420°C.Fig.2 shows an SEM image and the corresponding EDS maps of the sintered specimen after etching.As seen in the SEM image,the area of compositional change at the edge of the Mg sheet was thickly formed.As indicated by the EDS maps of Mg and Al,two phases were generated between Mg and Al in a layered state.In addition,the thickness of the Mg sheet was 250 μm before sintering,and the width of pure Mg after sintering was approximately 155 μm.This indicated Al and Mg diffused in an opposite direction.Numerous O spots were detected.These spots tended to be observed at the Mg sheet and Al powder locations.This is likely because Mg and Al surfaces are easily oxidized.The signals of Si spots were also seen,which are believed to be the result of contamination.Table 1 shows the relative concentrations (at.%) at Points 1 and 2 in Fig.2.At Point 1,the Mg was 56 at.% and the Al was 39 at.%,respectively.At Point 2,the Mg was 42 at.% and the Al was 56 at.%.As predicted,the Mg concentration of Point 1 was found to be higher than that of Point 2.In addition,the Al concentration was higher at Point 2 than at Point 1.It is anticipated that Al and Mg interdiffusion occurred during the SPS process.

    In order to evaluate the formation of theβphase(Mg17Al12),the atomic ratios of Mg/Al at Points 1 and 2 were recorded in Table 1.According to binary phase diagrams of Mg-Al [49–53],theβphase has an atomic ratio of Mg/Al between 0.82 and 1.73.This ratio was reported to beca.2 for die-cast AZ91D Mg alloy [33].Therefore,the range of 0.82 to 2 indicates the potential formation of theβphase.Similarly,the Mg/Al atomic ratios of 0.65 to 0.74 indicate the formation of theγphase (Mg2Al3).According to Table 1,the Mg/Al ratio at Point 1 was 1.44,and at Point 2 it was 0.75.These results suggest that Point 1 was in theβphase,whereas Point 2 was most likely in theγphase.Whether or not the area at Point 1 is aβphase will be determined in detail later;however,for simplicity,the area with an Mg/Al ratio of 0.8–2 is referred to as theβphase.

    Table 1 Relative concentrations (at.%) and atomic ratios of Mg/Al at Points 1 and 2 in Fig.2.

    Table 2 Relative concentrations (at.%) and atomic ratios of Mg/Al at Points 3–8 in Fig.3.

    According to our preliminary research,Mg would melt and adhere to graphite punches when the sintering temper-ature was set to 430 °C.In addition,it was confirme that theβphase did not form at lower temperatures.Therefore,the sintering temperature of 420 °C was determined to be appropriate.To generate a singleα/βphase boundary,it is necessary to prevent the formation of theγphase.This topic will be discussed in the subsequent section.

    Fig.2.SEM image and the corresponding EDS maps of the etched specimen sintered from an Mg sheet,surrounded by Al powders kept at 420 °C for 30 min.

    3.1.2.Optimizing fabrication conditions

    Fig.3.SEM images and the corresponding EDS maps of the etched specimens sintered from a 0.10 mm thick Al foil surrounded by Mg powders at 420 °C for (a) 50 min,(b) 80 min,and (c) 120 min.

    As a second step,the layer pattern shown in Fig.1 was utilized for sintering: a 0.10 mm thick Al foil was used for Layer 3,and 0.23 g of Mg powder was used for Layers 2 and 4,respectively.Fig.3 shows SEM images and the corresponding EDS maps of sintered specimens after etching.The temperature was set to 420 °C and the holding time was increased from 50 min to 120 min.As shown in Fig.3a and 3b,when the holding time was 50 min (Fig.3a) and 80 min(Fig.3b),a central portion of the Al foil remained as pure Al.The Mg and Al maps exhibited color gradients,indicating the diffusion of Mg and Al.EDS point analysis confirme the formation of theβphase (Mg17Al12) andγphase (Mg2Al3);the results are shown in Table 2.As seen in Table 2,the Mg/Al atomic ratio was 0.69 at Point 3 and 1.48 at Point 4 in Fig.3a(50 min).According to these results,Point 3 was in theγphase and Point 4 was in theβphase.Since theβphase has a lower Al concentration than theγphase,it is reasonable that theβphase is further away from the Al foil than theγphase.At Points 5 and 6 in Fig.3b (80 min),the atomic ratio of Mg/Al was 0.72 and 1.31,respectively.According to these results,Point 5 was in theγphase and Point 6 was in theβphase.The thickness of theβphase fabricated for 50 min and 80 min exhibited no discernible difference,whereas the atomic ratio of Mg/Al increased slightly for 80-min sintering.

    Table 3 Relative concentrations (at.%) and atomic ratios of Mg/Al at Points 9–11 in Fig.4.

    As shown in Fig.3c,when the holding time was extended to 120 min,the remaining pure Al disappeared and dense lamellar structures were formed.As the sintering time grew longer,it is possible that theβphase melted during the SPS process.Accordingly,it was believed that lamellar structures emerged.At Points 7 and 8,the Mg/Al atomic ratio was 1.18 and 0.74,respectively.According to these results,Point 7 was in theβphase and Point 8 was in theγphase.By increasing the sintering time from 80 min to 120 min,the remaining Al disappeared,but theγphase remained.These results are likely attributable to an excessive amount of Al relative to Mg.Based on research indicating that the growth rate of theγphase is faster than that of theβphase,this expectation seems reasonable [54,55].Consequently,reducing the amount of Al may be more effective than adjusting the holding time.

    As the next step,a 0.05 mm Al foil was used for Layer 3,while 0.23 g of Mg powder was used for Layers 2 and 4,respectively.The 50-min sintering was performed at 420 °C.Fig.4 shows an SEM image and the corresponding EDS maps of the sintered specimen after etching.As shown in the EDS maps,a microstructure with Mg and Al concentration gradients was generated.A comparison between the SEM image and the EDS map of Al reveals that the dark gray area of this microstructure contains a higher concentration of Al than the lighter gray areas.In addition,according to Table 3,the composition at Point 9 was 64 at.% Mg and 35 at.% Al,whereas at Point 10,the composition was 48 at.% Mg and 44 at.% Al.At these two points,the Mg/Al atomic ratio was 1.83 and 1.10.These values fall within the range indicative ofβphase formation.Consequently,a microstructure with gradations in Mg and Al concentrations was predicted to be predominantβphase;however,EDS data revealed that the distributions of Mg and Al were not uniform.The outer portion of the area with Mg and Al concentration gradients was believed to be theαphase with a relatively high Al concentration.In the SEM images,this area appears dark gray.Additionally,O signals were detected in this area.As shown in Fig.4,the signals of Fe were detected at the center of theβphase,and the concentration at Point 11 was 3 at.%.Thus,Fe was most likely a surface impurity introduced during the rolling process of the Al foils.Since Fe-containing intermetallic particles may serve as corrosive cathode sites in the corrosion of Mg alloys,these particles are expected to impede the analysis of corrosion behavior [56,57].Therefore,an Al starting raw material with low Fe impurity is necessary.

    Fig.4.SEM images and the corresponding EDS maps of the etched specimen sintered from a 0.05-mm-thick Al foil surrounded by Mg powders kept at 420°C for 50 min.

    In the subsequent step,instead of Al foils,a pre-pressed Al powder layer (purity: 99.99%) was used as Layer 3,and Mg powders (0.23 g) were used as Layers 2 and 4,respectively.The amount of Al powders was 0.024 g,which is equal to one Al foil measuring 0.05 mm in thickness.The sintering was conducted for 70 min at 420 °C.After etching,the sintered specimen is depicted in Fig.5 with the SEM image and the corresponding EDS maps.Pure Al areas remained when the holding time was set to 50 min,which was the same as the sintering time for specimens made with 0.05 mm foils;therefore,the holding time was set to 70 min.This could be due to the uneven pressing of Al powders in the SPS die.Table 4 shows the relative concentrations at Points 12–15 in Fig.5.At each of these points,Fe concentrations were less than 0.01 at.%.In this instance,a microstructure with a concentration gradient of Mg and Al was also fabricated.Points 14 and 15 of the EDS point analysis were examined.According to Table 4,the Mg/Al atomic ratios at Points 14 and 15 belonged to theβphase range.At Point 12,the relative concentration of Al was 0.4 at.%,which corresponds to theαphase (primaryαphase) of Mg-Al alloys.In contrast,the concentration of Al at Point 13 was 7 at.%.It suggested that this area was Al-enrichedαphase.Depending on the distance from the region of Al powder,the concentration of Al in the other point analyses varied betweenca.7 at.% toca.10 at.%.This area most likely corresponds to the region occasionally observed near the grain boundaries of as-cast AZ91,which is identifie as the eutecticαphase with a higher Al content than the primaryαphase [23,58].

    Fig.5.SEM images and the corresponding EDS maps of the etched specimen sintered from a pre-pressed Al powder layer (equal to 0.05-mm-thick Al foil)surrounded by Mg powders kept at 420 °C for 70 min.

    Table 4 Relative concentrations (at.%) and atomic ratios of Mg/Al at Points 12–15 in Fig.5.

    Fig.6.(a) BSE image of the specimen shown in Fig.5 and (b) changes in the atomic concentrations and atomic ratios of Mg and Al with distance.

    3.2.Phase identificatio

    To clearly determine the formation of theβphase,electron probe micro analyzer (EPMA),X-ray diffraction (XRD),and scanning transmission electron microscopy(STEM)were conducted.Fig.6a shows a back-scattered electron (BSE) image of the specimen shown in Fig.5.The white line indicates the location of the EPMA analysis,and Fig.6b shows the changes in the atomic concentrations and atomic ratios of Mg and Al with distance.0 μm represents the left side of the white line drawn in Fig.6a.In Fig.6b,from 0 to 35 μm,the atomic concentration of Mg decreased gradually,whereas that of Al increased gradually from 3 at.% to 11 at.%.In the range between 35 and 40 μm,the atomic concentration of Mg decreased sharply,while that of Al increased sharply from 11 at.% to 35 at.%.In the range of 40 μm to 66 μm denoted by the dotted rectangle,the atomic concentrations of Mg and Al were stable,and the Mg/Al atomic ratio ranged from 1.85 to 1.42,indicating the formation of theβphase.In addition,Al-enrichment was observed in the region between 15 and 40 μm.This region appears to correspond to the eutectic phase of Mg-Al alloys and contains the Al-enrichedαphase.

    Fig.7 illustrates the XRD pattern of the specimen shown in Fig.5.The rhombuses represent the peaks of theβphase(Mg17Al12).In addition,there were peaks of Al andαphase of Mg.Al peaks were detected because the outermost layers(Layers 1 and 5) of the sintered specimen were composed of Al powders.As shown in Fig.7,the intensity of theβphase peaks was low.This is due to the fact that the formation of theβphase is restricted to the boundary between the layers of Mg and Al powders.

    Fig.7.X-ray diffraction pattern of the specimen shown in Fig.5.

    Figs.8a and 8b show an annular bright-fiel (ABF) image of a cross-section of theβphase shown in Fig.5.The cross-section was fabricated by a focused ion beam (FIB).Fig.8c shows the electron diffraction pattern.Accordingly,it was categorized asβphase(Mg17Al12,bcc,a=1.05438 nm).On the basis of current findings it can be concluded that the boundary between theαphase andβphase was successfully fabricated.

    3.2.Optimal SPS parameters for α/β boundary formation

    The sintering temperature is,in general,the most important variable in SPS processing.Some researchers have hypothesized that extremely high temperatures are necessary for the formation of theβphase from the mixed Mg and Al powders[55,59,60].However,in this study,sintering at 420 °C led to the formation of a singleα/βphase boundary.In addition to temperature,an oxide fil on Al powders has occasionally become the center of attention [61].At low sintering temperatures,it is difficul to break down the native oxide fil and maintain metal/oxide/metal bonds [62–64].Thus,diffusion of Al and the formation of theβphase are challenging.Additionally,diffusion is slow at low temperatures.Therefore,high temperatures are suitable for the formation of a singleα/βphase boundary.In contrast,some researchers asserted that the amount ofβphase decreased as the temperature was increased [65],and it was reported that temperatures below 360 °C were advantageous for the formation of theβphase[66].Further study is required to identify the SPS temperature that suppresses the formation of theγphase and efficientl fabricates theα/βboundary.

    Fig.8.(a,b) STEM images and (c) diffraction pattern of the β phase shown in Fig.5.

    In addition,it is well known that SPS typically has a short sintering time,but the holding time observed in this study was relatively long.However,a long holding time was necessary to fabricate a singleα/βphase boundary(see supplemental 1).In addition,this study revealed that the amount of Al (Layer 3) was a crucial factor in forming theβphase and preventing the formation of theγphase.This is because theβphase(Mg17Al12) is the second phase in the Mg-Al alloy system with the lowest Al content.In the process of alloying Mg and Al powders,the presence of excess Al results in the formation of theγphase,which is located on the Al-rich side of the Mg-Al binary diagrams.Thus,to obtain a singleα/βphase boundary,the quantity of Al powders must be precisely controlled (see supplemental 2).

    This study demonstrated that a singleα/βphase boundary can be fabricated by sintering Mg powders and a small amount of Al powders at 420 °C for 70 min.The change in Al concentration from theαphase to theβphase depicted in Fig.6 is comparable to that reported in the literature for AZ91D [67],so it can be concluded that the specimen simulating a singleα/βboundary in AZ91 was successfully fabricated in this study.In addition,we were able to fabricate anαphase containing supersaturated Al on theβphase side of theαphase,which corresponds to the eutecticαphase.

    3.4.In situ observations of galvanic corrosion at the α/β phase boundary

    3.4.1.Open-circuit potential of each phase

    To ascertain micro-galvanic coupling behavior at theα/βphase boundary of Mg-Al alloys,the open-circuit potentials(OCPs) of a small area composed ofαphase,βphase,and theα/βphase boundary (αandβphases) were measured,respectively.Fig.9 shows optical microscope images of the electrode areas before and after OCP measurements.Fig.10 shows the time variations of the OCPs of each specimen in naturally aerated 0.1 M NaCl at pH 8.0 (25 °C).The electrode of theαphase was made at least 50 μm away from theβphase to avoid the Al-enriched area.The electrode of theβphase was made at least 10 μm away from theβphase boundaries.The area of the Al-enrichedαphase was about 25 μm in the electrode of theα/βphase boundary.In addition,Figs.11,12,and 13 show optical microscope images of the electrode area of theαphase,theβphase,and theα/βphase boundary,respectively.The labels “a1–11”,“a2–l2”,and“a3–13” in Fig.10 correspond to the images (a) through (l)in Figs.11,12,and 13,respectively.The time-lapse images in Figs.11,12,and 13 were extracted from the movie during the OCP measurements.To facilitate comparison,the images for each label are displayed simultaneously for all three specimens.In Figs.11,12,and 13,“0 s” indicates immediately after immersion.

    As seen in Fig.9a and 9b,corrosion (discoloration) occurred on both theαphase andβphase electrode areas.Also,in the case of the specimen with theα/βphase boundary,discoloration was generated.In Fig.9c,the left side of the image was theβphase,while the right side was theαphase.Accordingly,the left side of theαphase and the left side of theβphase were discolored.As shown in Fig.10,the OCPs were initially low and then increased to approximately?1.6 V in all cases.However,a closer inspection of the particulars reveals the unique characteristics of each specimen.During the initial stage of immersion,theβphase specimen exhibited a higher potential than theαphase specimen.The observation that theβphase exhibited higher OCP than theαphase is consistent with previous finding [68–70].Lunder et al.[32] reported that the corrosion potential of–1.66 VSCEfor Mg and ?1.2 VSCEforβphase in 5% NaCl saturated with Mg(OH)2.Interestingly,as shown in Fig.10,the small area composed ofαphase andβphase exhibited intermediate values.A micro-galvanic cell was likely to form between theαandβphases in 0.1 M NaCl.

    3.4.2.Corrosion behavior of α phase,β phase,and α/β phase boundary

    Fig.9.Optical microscope images of the electrode areas before and after OCP measurements.The electrode areas compose of (a) α phase,(b) β phase,and (c) α and β phases (α/β phase boundary).The images in the left and right columns are the electrode areas before and after the OCP measurements,respectively.

    During the OCP measurement,the optical microscope images shown in Fig.11 are surface appearances of the electrode area composed ofαphase.In this instance,the electrode area was made at least 80 μm away from theβphase;therefore,the Al concentration is estimated to be less than 3 at.% based on Fig.6b.As shown in Fig.11,gas bubbles (probably H2gas) were observed at the beginning of immersion,but significan corrosion (discoloration) did not occur until 40 s.At 60 s,the discoloration was clearly visible in the lower right portion of the electrode area,and the degree of discoloration increased until 200 s.At 300 s,the discoloration almost spread across the entire electrode area,and the degree of discoloration thereafter increased with time.Comparing the spreading behavior of discoloration to the time variation of the OCP,it was discovered that between 200 s and 300 s,when the discoloration spread across the entire surface,the OCP increased significantl and then stabilized atca.?1.6 V.

    As shown in Fig.12,the corrosion and discoloration behaviors of theβphase were significantl distinct from those of theαphase.In contrast,no bubbles were generated.Moreover,the degree of discoloration of theβphase was less than that of theαphase.However,the upper and lower portions of the electrode were slightly discolored immediately after immersion.From 10 to 100 s,the degree of discoloration intensifie gradually from light brown to dark brown.Throughout this time period,the OCPs increased from ?1.67 V to?1.57 V.At 200 s,the discolored area turned to a lighter brown.At 600 s,the light brown discoloration was found to spread across the entire surface.As stated previously,a comparison of Figs.11 and 12 reveals that the discoloration(corrosion) of theβphase was slight compared to that of theαphase.Probably due to the formation of a corrosionresistant fil on the surface of theβphase,the OCPs of theβphase were higher than that of theαphase [71].It may be related to the high potential ofβphase and the slight discoloration.A small pit was initiated at the location indicated by the blue arrow in the discolored area,and it grew slowly.This is presumed to have caused the potential oscillations after 200 s.

    Fig.10.Time variations of the OCPs of each specimen in naturally aerated 0.1 M NaCl solution at pH 8.0 (25 °C).The electrode areas compose of(a) α phase,(b) β phase,and (c) α and β phases (α/β phase boundary),as shown in Fig.9.Labels “a1” to “l(fā)1” correspond to the images in Fig.11.Labels “a2” to “l(fā)2” correspond to the images in Fig.12.Labels “a3” to “l(fā)3”correspond to the images in Fig.13.

    For the electrode area comprised ofαphase andβphase,as shown in Fig.13,gas bubbles were generated immediately after immersion.However,the bubble generation positions were not in theβphase,but in theαphase.At 10 s,the color of theβphase was observed to change to light brown.Thereafter,the discoloration of theβphase became gradually darker until 300 s.Subsequently,the discoloration of theβphase faded over time.Additionally,discoloration was observed in theαphase.The right side of theαphase began to turn light brown at 40 s.The discoloration of theαphase became gradually darker over time,but it did not significantl expand.In this experiment,the area of discoloration in theαphase was restricted to the right side of the electrode surface,while the middle portion of the electrode area remained unaffected.This region corresponds to the cathode of the micro-galvanic cell between theαandβphases.In Mg-Al alloys,it is proposed thatβphases serve as preferential cathodes,whereasαphases are primarily responsible for anodic reactions [25–28].As shown in Fig.10,the OCP of theβphase was higher than that of theαphase,so theβphase would serve as the cathode under natural immersion conditions.However,it was anticipated that the micro-galvanic corrosion behavior would be more complex,and it was discovered that the generation of gas bubbles did not occur in theβphase within 10 min,but rather in theαphase close to theβphase.Theαphase,which is close to theβphase,was anticipated to be a cathode during microgalvanic corrosion between theαandβphases at least in the initial stage of immersion.In Mg alloys,it was generally believed that theβphase mainly serves as a galvanic cathode and accelerates the corrosion of theα-Mg matrix.However,we found that theβphase was not always the preferred cathode in micro-galvanic corrosion of theαphase and theβphase.

    Fig.11.Optical microscope images of the electrode area composed of the α phase during the OCP measurement.Each of the images (a)–(l) is taken at the time marked as “a1”–“l(fā)2” indicated by the black dots in Fig.10.

    Fig.12.Optical microscope images of the electrode area composed of the β phase during the OCP measurement.Each of the images (a)–(l) is taken at the time marked as “a2”–“l(fā)2” indicated by the black dots in Fig.10.The blue arrow indicated a small pit.

    3.4.3.Long-time OCP measurement of α/β phase boundary

    To further clarify the micro-galvanic corrosion behavior of theα/βphase boundary,a long-time immersion(1 h)was carried out in naturally aerated 0.1 M NaCl at pH 8.0 (25 °C).Fig.14 shows the time variations of the OCP,and Fig.15 illustrates optical microscope images of theα/βboundary in the electrode area during immersion.The left side of the electrode area in Fig.15 was theβphase,while the right side was theαphase.The labels “a–1” in Fig.14 correspond to the images of (a) to (l) in Fig.15.As shown in Fig.14,the OCP oscillated and increased from ?1.73 V to ?1.55 V.

    As shown in Fig.15a,gas bubbles were generated immediately after immersion,and in this instance,gas bubbles were also observed in theαphase near theβphase.In the initial stage of immersion,theαphase,which is close to theβphase,was thought to become a cathode even under micro-galvanic coupling between theαandβphases.Since gas bubbles were observed on theαphase side of theα/βboundary at 0 s,it was determined that a galvanic cell formed between theβphase andαphase on the electrode area.However,no bubbles were observed in theβphase,indicating that H2gas generation onβphase of Mg-Al alloys is unlikely.According to previous research,the cathodic activity ofβphase is relatively low compared to that of theαphase [32,74,75].Moreover,the potential difference between theβphase and the Mg-matrix (αphase) was in the range of 10 mV,which was insufficien to form a strong galvanic couple,according to the previous research [29,76].These are presumed to be the causes of the absence of bubbles in theβphase.

    Fig.13.Optical microscope images of the electrode area composed of the α/β phase during the OCP measurement.Each of the images (a)–(l) is taken at the time marked as “a3”–“l(fā)3” indicated by the black dots in Fig.10.

    Fig.14.Time variations of the OCP of a small area composed of the α and β phases (α/β phase boundary) in naturally aerated 0.1 M NaCl solution at pH 8.0 (25 °C).Labels “a”–“l(fā)” correspond to the images in Fig.15.

    In Fig.15a (0 s),theβphase has already discolored to faint brown color.This discoloration gradually disappeared after 40 s.At 40 s,the right side of theαphase began to discolor.Subsequently,the discolored area on theαphase expanded toward theβphase.Even after 1 h of immersion,not all of theαphase discolored,and theαphase withinca.50 μm of theα/βphase boundary remained uncolored.As the discoloration of theαphase approached theβphase,bubbles were generated in theβphase.Therefore,it appears that theβphase does not serve as the preferred cathode.In contrast,theαphase partially corrodes (or discolors) and becomes the anodes,whereas the surrounding areas are most likely to be the cathodes.In other words,theαphase can function as a cathode,and theβphase would function as a cathode if corroded areas (anodes) in theαphase approached theβphase.During the initial stage of immersion in this study (Figs.13 and 15),the discoloration occurred in theαphase was 300 μm away from theβphase,where it became the anode;consequently,theβphase likely did not initially become the cathode.If the size of theαphase is smaller than that used in this study,there is a possibility that theβphase could have served as the cathode from the start of the immersion.

    Fig.15.Optical microscope images of a small area composed of α and β phases (α/β phase boundary) during the long-time immersion (1 h).

    Fig.16.(a) SEM image of the as-polished specimen surface with α/β phase boundary and (b–d) AES depth profiles (b) β phase,(c) β phase near the boundary of α phase,(d) Al-rich α phase,and (e) α phase without Al-enrichment.The indentations were made to confir the analyzed positions.

    In Fig.15l,theαphase withinca.50 μm of theα/βphase boundary remained without discoloration even after 1 h of immersion.This region is determined to be the Al-enrichedαphase based on Fig.6.Accordingly,the corrosion resistance of the Al-enrichedαphase was determined to be higher than that of theαphase without Al-enrichment.According to reports,the corrosion and/or dissolution rate of Mg-Al alloys decreases as Al concentration increases [72,73].The observed discoloration behavior at and around theα/βphase boundary is consistent with these findings

    3.5.Surface fil on each phase

    Auger electron spectroscopy (AES) was used to determine why the Al-enrichedαphase exhibits a higher corrosion resistance than the phase without Al-enrichment.The specimen was etched,then slightly polished,and placed in the AES chamber on the same day.Fig.16a is a SEM image showing the analyzed positions on the as-polished specimen with theα/βphase boundary.AES depth profile were obtained on 1)βphase,2)βphase nearαphase,3) Al-enrichedαphase,and 4)αphase without Al-enrichment.As shown in Fig.15b through 15e,the O signal was detected on the surface in all areas.The oxide fil thickness was calculated as half of the sum of the maximum and minimum values of O Despite the fact that the specimen was sputtered deeply,the O concentration did not reach zero;therefore,the thickness indicated in Fig.15 is a reference value.Regardless,the expected order of fil thickness is as follows: (thick)αphase without Al-enrichment>Al-enrichedαphase>βphase ≈βphase nearαphase (thin).This order of thickness is consistent with the order of Al concentration in the oxide films The finding indicate that Al inhibits the formation of surface oxide film in air.

    Fig.17a and 17b show an optical microscope image and SEM image of the electrode area with theα/βphase boundary after the OCP measurement(10 min immersion)as shown in Fig.13.Also in this instance,AES depth profile were acquired on 1)βphase (discolored),2)βphase nearαphase(non-discolored),3) Al-enrichedαphase (non-discolored),and 4)αphase without Al-enrichment (discolored),and the thickness of the oxide fil at each point was calculated using the same method as in Fig.16.By comparing Figs.17 and 16 (notice the difference in the range of the horizontal axis),it was confirme that oxide film grew by immersion.The surface oxide film on the discoloredβphase and the discoloredαphase without Al-enrichment were relatively thick.In contrast,the surface oxide film were relatively thin on theβphase adjacent to theαphase (non-discolored) and the Alenrichedαphase (non-discolored).A high Al concentration oxide fil was formed on the Al-enrichedαphase compared to theαphase without Al-enrichment,as depicted in Figs.17e and 17f.Therefore,it may be concluded that Al in the surface oxide fil suppressed the corrosion and/or discoloration in the Al-enrichedαphase.

    In Figs.13 and 15,the discoloration on theβphase in the initial stage of immersion disappeared with time,which may be due to the dissolution of the corrosion products by the alkalization resulting from the cathodic reaction,but the details are unknown.

    4.Conclusions

    1.A specimen with a single boundary ofα/βphase simulating Mg-Al alloys was successfully fabricated using SPS.Al enrichment was also observed on theαphase side of the boundary,which appeared to correspond to the eutecticαphase of Mg-Al alloys.

    2.The OCPs of each phase and a small area with the boundary in 0.1 M NaCl at pH 8.0 were compared:theβphase exhibited a higher potential,whereas theαphase exhibited a lower potential.The OCP of a small area containing theα/βphase boundary was the intermediate value of these phases.

    3.Under natural immersion of the 0.1 M NaCl solution,discoloration and gas bubble generation were observed on a small area of theαphase,whereas no bubble generation was observed on theβphase.In the case of a small area with anα/βphase boundary,discoloration and gas bubbles were observed on theαphase,but no bubble generation was observed on theβphase.By long-time immersion as the discoloration (corrosion) of theαphase approached theβphase,the bubbles were generated on theβphase.

    4.In micro-galvanic corrosion of theαphase and theβphase,it was determined that theβphase was not always the preferred cathode.Theαphase partially corroded (or discolored) and became the anodes,whereas the surrounding areas were likely to be the cathodes.When corroded areas (anodes) of theαphase approached theβphase,theβphase would become the cathodes.

    5.Even after 1 h of immersion in the 0.1 M NaCl solution,the Al-enriched phase located close to theα/βphase boundary exhibited no discoloration.Al in the surface oxide fil inhibited corrosion and/or discoloration in the Al-enrichedαphase.

    Data availability

    The raw/processed data required to reproduce these find ings cannot be shared at this time because the data also forms part of an ongoing study.

    Declaration of Competing InterestThe authors declare that they have no known competing financia interests or personal relationships that could have appeared to influenc the work reported in this paper.

    CRediT authorship contribution statementZheng Shao:Investigation,Data curation,Methodology,Writing– original draft.Masashi Nishimoto:Data curation,Writing– review &editing.Izumi Muto:Conceptualization,Methodology,Writing– review &editing,Supervision,Funding acquisition.Yu Sugawara:Writing– review &editing.

    Acknowledgments

    Part of this work was supported by JSPS KAKENHI Grant Numbers JP17H01331 and JP21K18804.This study was supported by The Light Metal Educational Foundation Inc.of Japan.This research was also supported by Amano Institute of Technology and China Scholarship Council.

    Supplementary materials

    Supplementary material associated with this article can be found,in the online version,at doi:10.1016/j.jma.2022.10.020.

    法律面前人人平等表现在哪些方面| 男女高潮啪啪啪动态图| 免费在线观看日本一区| 黄网站色视频无遮挡免费观看| 免费少妇av软件| 99精国产麻豆久久婷婷| 日本vs欧美在线观看视频| 黄片播放在线免费| 老汉色∧v一级毛片| 精品人妻1区二区| 精品人妻在线不人妻| 波多野结衣av一区二区av| 伊人久久大香线蕉亚洲五| 777久久人妻少妇嫩草av网站| 黄色a级毛片大全视频| 久久久久久亚洲精品国产蜜桃av| 欧美日韩亚洲综合一区二区三区_| 精品乱码久久久久久99久播| 国产精品久久久av美女十八| 亚洲视频免费观看视频| 久久精品91无色码中文字幕| 欧美中文综合在线视频| 我的亚洲天堂| 91大片在线观看| 制服人妻中文乱码| 两人在一起打扑克的视频| 精品国产一区二区久久| av片东京热男人的天堂| 免费在线观看亚洲国产| 性少妇av在线| 亚洲男人的天堂狠狠| 丰满人妻熟妇乱又伦精品不卡| 两个人看的免费小视频| 精品国产乱子伦一区二区三区| 男男h啪啪无遮挡| 亚洲成人久久性| 两个人免费观看高清视频| 久久精品国产亚洲av高清一级| 久久久久久亚洲精品国产蜜桃av| 一边摸一边抽搐一进一出视频| 国产在线观看jvid| 国产精品久久久久久人妻精品电影| 国产成人欧美在线观看| 9热在线视频观看99| 亚洲成人精品中文字幕电影 | 99香蕉大伊视频| 一级毛片女人18水好多| 神马国产精品三级电影在线观看 | 国产精品电影一区二区三区| 久久人人97超碰香蕉20202| 19禁男女啪啪无遮挡网站| 久久精品亚洲av国产电影网| 亚洲色图综合在线观看| 午夜免费成人在线视频| 欧美成人性av电影在线观看| 日本三级黄在线观看| 午夜激情av网站| 国产野战对白在线观看| 国产一卡二卡三卡精品| 在线免费观看的www视频| 国产高清激情床上av| 一级a爱视频在线免费观看| 9191精品国产免费久久| 夜夜躁狠狠躁天天躁| 在线av久久热| 中出人妻视频一区二区| 国产精品亚洲av一区麻豆| 亚洲欧美日韩高清在线视频| 亚洲精品中文字幕在线视频| 90打野战视频偷拍视频| 大码成人一级视频| 又黄又爽又免费观看的视频| 亚洲国产看品久久| 啦啦啦 在线观看视频| 电影成人av| 多毛熟女@视频| 在线观看66精品国产| 国产免费av片在线观看野外av| 18美女黄网站色大片免费观看| 国产精品 欧美亚洲| 亚洲欧美精品综合一区二区三区| 天堂动漫精品| 桃色一区二区三区在线观看| 国产乱人伦免费视频| 午夜福利一区二区在线看| 中国美女看黄片| av天堂久久9| 精品一区二区三区视频在线观看免费 | 午夜福利欧美成人| 母亲3免费完整高清在线观看| 国产精品久久电影中文字幕| 一区二区三区激情视频| 亚洲av电影在线进入| aaaaa片日本免费| 欧美日韩国产mv在线观看视频| 涩涩av久久男人的天堂| 久久亚洲真实| 99久久精品国产亚洲精品| 亚洲avbb在线观看| 欧美日韩一级在线毛片| 久久久水蜜桃国产精品网| 欧美在线黄色| 精品国产一区二区三区四区第35| 亚洲精品国产区一区二| 免费在线观看影片大全网站| 神马国产精品三级电影在线观看 | 久久香蕉精品热| 女人被躁到高潮嗷嗷叫费观| 天天影视国产精品| 免费av毛片视频| 黑丝袜美女国产一区| 在线观看免费日韩欧美大片| 女人被狂操c到高潮| av国产精品久久久久影院| 99国产精品一区二区三区| 亚洲精品中文字幕在线视频| 啦啦啦免费观看视频1| 黄片小视频在线播放| 叶爱在线成人免费视频播放| 亚洲精品国产精品久久久不卡| 国产成人一区二区三区免费视频网站| 久久精品亚洲av国产电影网| 操美女的视频在线观看| 老司机午夜福利在线观看视频| 日本wwww免费看| 99香蕉大伊视频| bbb黄色大片| 在线av久久热| 婷婷丁香在线五月| 成人18禁在线播放| 香蕉久久夜色| 在线观看一区二区三区| 中文字幕人妻熟女乱码| 免费av中文字幕在线| 免费一级毛片在线播放高清视频 | 在线观看免费日韩欧美大片| 亚洲一区高清亚洲精品| 精品国产乱子伦一区二区三区| 久久久久久人人人人人| 国产精品久久久久久人妻精品电影| 国产aⅴ精品一区二区三区波| 国产视频一区二区在线看| 国产欧美日韩精品亚洲av| x7x7x7水蜜桃| 女性被躁到高潮视频| 国产精品久久久人人做人人爽| 青草久久国产| 亚洲av片天天在线观看| 久久天堂一区二区三区四区| 日本撒尿小便嘘嘘汇集6| 色婷婷久久久亚洲欧美| 日本精品一区二区三区蜜桃| 中出人妻视频一区二区| 老熟妇仑乱视频hdxx| 精品国产乱码久久久久久男人| 久久伊人香网站| 黄色 视频免费看| 免费高清在线观看日韩| 亚洲欧洲精品一区二区精品久久久| 麻豆久久精品国产亚洲av | www日本在线高清视频| 另类亚洲欧美激情| 三级毛片av免费| 色婷婷久久久亚洲欧美| 久久香蕉国产精品| 久久伊人香网站| 久久久久久人人人人人| 最近最新免费中文字幕在线| 亚洲精品av麻豆狂野| 国产成人欧美| 亚洲精品久久成人aⅴ小说| 午夜福利,免费看| 美女高潮到喷水免费观看| 欧美日韩亚洲综合一区二区三区_| 18禁美女被吸乳视频| 精品福利永久在线观看| 免费看十八禁软件| 免费在线观看亚洲国产| 黄色怎么调成土黄色| 天堂俺去俺来也www色官网| 99国产精品免费福利视频| x7x7x7水蜜桃| av免费在线观看网站| 亚洲熟妇熟女久久| 国产精品久久电影中文字幕| 久久人人97超碰香蕉20202| 久久99一区二区三区| 亚洲情色 制服丝袜| 91成人精品电影| 午夜免费激情av| 精品高清国产在线一区| 精品乱码久久久久久99久播| 老司机福利观看| 热re99久久精品国产66热6| 欧美日韩亚洲综合一区二区三区_| 久久久久精品国产欧美久久久| 999久久久国产精品视频| 欧美成人性av电影在线观看| 国产成人精品久久二区二区免费| 另类亚洲欧美激情| 可以免费在线观看a视频的电影网站| 亚洲中文字幕日韩| 狠狠狠狠99中文字幕| 亚洲在线自拍视频| 一区福利在线观看| 欧美丝袜亚洲另类 | 侵犯人妻中文字幕一二三四区| 美女高潮到喷水免费观看| 美女扒开内裤让男人捅视频| 99久久人妻综合| 中亚洲国语对白在线视频| 成人精品一区二区免费| 免费在线观看完整版高清| av片东京热男人的天堂| 国产高清视频在线播放一区| 国产成人影院久久av| 午夜91福利影院| 国产91精品成人一区二区三区| 免费在线观看亚洲国产| 一边摸一边做爽爽视频免费| 69av精品久久久久久| 窝窝影院91人妻| 在线视频色国产色| 真人一进一出gif抽搐免费| 日本精品一区二区三区蜜桃| 免费在线观看亚洲国产| 成人特级黄色片久久久久久久| 成人亚洲精品一区在线观看| 级片在线观看| ponron亚洲| 亚洲欧美一区二区三区黑人| 国产99久久九九免费精品| 久久久国产欧美日韩av| 麻豆国产av国片精品| 亚洲av成人一区二区三| 午夜福利,免费看| 色婷婷av一区二区三区视频| 国产99白浆流出| 丝袜美腿诱惑在线| 91老司机精品| 国产一区在线观看成人免费| 国产精品美女特级片免费视频播放器 | avwww免费| 十八禁网站免费在线| 在线观看免费视频网站a站| 国产av一区二区精品久久| 岛国视频午夜一区免费看| 欧美激情 高清一区二区三区| 国产精品久久久久久人妻精品电影| √禁漫天堂资源中文www| 国产精品一区二区精品视频观看| avwww免费| 久久99一区二区三区| 91麻豆av在线| 热99国产精品久久久久久7| 国产不卡一卡二| 99国产综合亚洲精品| 别揉我奶头~嗯~啊~动态视频| 我的亚洲天堂| 成人av一区二区三区在线看| 女性生殖器流出的白浆| 69精品国产乱码久久久| 制服人妻中文乱码| 中出人妻视频一区二区| 国产精品一区二区精品视频观看| 在线永久观看黄色视频| 亚洲人成电影观看| 脱女人内裤的视频| 99久久人妻综合| 日日干狠狠操夜夜爽| 最近最新中文字幕大全电影3 | 一二三四社区在线视频社区8| 精品熟女少妇八av免费久了| 又黄又粗又硬又大视频| 精品一品国产午夜福利视频| 国产精品久久视频播放| 久久青草综合色| 精品人妻1区二区| 日本免费a在线| 国产高清videossex| 色哟哟哟哟哟哟| 叶爱在线成人免费视频播放| 操出白浆在线播放| 丝袜美足系列| 国产xxxxx性猛交| 午夜免费激情av| 中文字幕av电影在线播放| 麻豆久久精品国产亚洲av | 亚洲成国产人片在线观看| 欧美人与性动交α欧美软件| 婷婷六月久久综合丁香| 日韩高清综合在线| 亚洲情色 制服丝袜| 国产精品综合久久久久久久免费 | 亚洲国产精品sss在线观看 | 精品欧美一区二区三区在线| 欧美国产精品va在线观看不卡| 欧美黑人精品巨大| 一个人观看的视频www高清免费观看 | 久久香蕉国产精品| 天天添夜夜摸| 日韩有码中文字幕| 夜夜躁狠狠躁天天躁| 999久久久精品免费观看国产| 宅男免费午夜| 午夜免费激情av| 窝窝影院91人妻| 天天躁狠狠躁夜夜躁狠狠躁| 国产精品秋霞免费鲁丝片| 激情视频va一区二区三区| 男女之事视频高清在线观看| 成人影院久久| 老汉色∧v一级毛片| 精品免费久久久久久久清纯| 午夜成年电影在线免费观看| 亚洲熟女毛片儿| 天堂√8在线中文| 精品久久久久久电影网| 欧美乱色亚洲激情| 99热只有精品国产| 中文欧美无线码| 色播在线永久视频| 亚洲精品国产精品久久久不卡| 9色porny在线观看| 亚洲视频免费观看视频| 最新美女视频免费是黄的| 两个人免费观看高清视频| 欧美成人免费av一区二区三区| 亚洲av成人不卡在线观看播放网| 国产成人av教育| 日韩中文字幕欧美一区二区| 成人手机av| 亚洲欧美激情在线| www.www免费av| 日韩精品中文字幕看吧| 亚洲黑人精品在线| 国产精品乱码一区二三区的特点 | 亚洲一区二区三区欧美精品| 在线观看66精品国产| 夜夜爽天天搞| 变态另类成人亚洲欧美熟女 | 成熟少妇高潮喷水视频| 一a级毛片在线观看| av片东京热男人的天堂| 亚洲五月色婷婷综合| 久久久国产精品麻豆| 大码成人一级视频| 国产亚洲精品久久久久久毛片| 国产欧美日韩一区二区三| 欧美乱妇无乱码| 国产成+人综合+亚洲专区| 久久中文看片网| 成人亚洲精品一区在线观看| 人妻久久中文字幕网| 12—13女人毛片做爰片一| 欧美日韩乱码在线| 欧美久久黑人一区二区| 波多野结衣av一区二区av| tocl精华| 亚洲午夜理论影院| 精品国产美女av久久久久小说| 久9热在线精品视频| 无限看片的www在线观看| 日韩欧美一区视频在线观看| 在线观看日韩欧美| 欧美精品亚洲一区二区| 国产一区二区激情短视频| 多毛熟女@视频| 国产精品综合久久久久久久免费 | 国产深夜福利视频在线观看| 老鸭窝网址在线观看| 国产1区2区3区精品| 两个人免费观看高清视频| 亚洲欧美激情综合另类| 中文亚洲av片在线观看爽| 国产有黄有色有爽视频| 国产伦一二天堂av在线观看| 欧美成人性av电影在线观看| 美女国产高潮福利片在线看| av超薄肉色丝袜交足视频| 色老头精品视频在线观看| 久久99一区二区三区| www日本在线高清视频| 日日干狠狠操夜夜爽| 亚洲国产精品合色在线| 日韩人妻精品一区2区三区| 丝袜美足系列| 午夜福利一区二区在线看| 操出白浆在线播放| 不卡av一区二区三区| 国产成年人精品一区二区 | 热99国产精品久久久久久7| 日韩欧美国产一区二区入口| 国产av精品麻豆| 夜夜夜夜夜久久久久| 国产精品1区2区在线观看.| 十八禁网站免费在线| 国产麻豆69| 一本大道久久a久久精品| 国产不卡一卡二| 制服诱惑二区| 曰老女人黄片| 嫩草影院精品99| 国产日韩一区二区三区精品不卡| 免费看a级黄色片| 久久久久国内视频| 久久久久久久久中文| 日本 av在线| 97超级碰碰碰精品色视频在线观看| 精品一区二区三区视频在线观看免费 | 亚洲激情在线av| 久久草成人影院| 波多野结衣av一区二区av| 亚洲成国产人片在线观看| 国产又爽黄色视频| 级片在线观看| 国产高清激情床上av| 女人被狂操c到高潮| 国产成人欧美| 免费看十八禁软件| 国产免费男女视频| 99在线人妻在线中文字幕| av天堂久久9| avwww免费| 人妻久久中文字幕网| 91成人精品电影| 亚洲人成电影免费在线| 精品一区二区三区视频在线观看免费 | 国产亚洲精品久久久久5区| 日日夜夜操网爽| 免费av毛片视频| 中出人妻视频一区二区| 大型黄色视频在线免费观看| 十八禁人妻一区二区| 成年版毛片免费区| 亚洲狠狠婷婷综合久久图片| 国产99久久九九免费精品| 宅男免费午夜| 大码成人一级视频| 久久欧美精品欧美久久欧美| 亚洲人成电影观看| 不卡av一区二区三区| 国产欧美日韩精品亚洲av| 搡老乐熟女国产| 丁香欧美五月| 99香蕉大伊视频| 亚洲熟女毛片儿| 桃色一区二区三区在线观看| 国产熟女xx| 宅男免费午夜| 久久草成人影院| 婷婷精品国产亚洲av在线| 亚洲人成电影观看| 国产精品一区二区精品视频观看| 黄频高清免费视频| 久久热在线av| 国产精品香港三级国产av潘金莲| 久99久视频精品免费| 水蜜桃什么品种好| 亚洲性夜色夜夜综合| 久久热在线av| 神马国产精品三级电影在线观看 | 欧美日韩亚洲综合一区二区三区_| 亚洲欧洲精品一区二区精品久久久| 免费在线观看完整版高清| 看片在线看免费视频| 少妇裸体淫交视频免费看高清 | 久久精品影院6| 9191精品国产免费久久| cao死你这个sao货| 精品一区二区三区视频在线观看免费 | 最近最新中文字幕大全电影3 | 亚洲精品在线美女| 99久久精品国产亚洲精品| 日韩精品免费视频一区二区三区| 国产成人啪精品午夜网站| 男人舔女人下体高潮全视频| 欧美中文日本在线观看视频| 欧美一区二区精品小视频在线| 18美女黄网站色大片免费观看| 国产精品国产高清国产av| 亚洲狠狠婷婷综合久久图片| 免费在线观看日本一区| 日韩欧美三级三区| 国产av一区在线观看免费| 婷婷精品国产亚洲av在线| 波多野结衣一区麻豆| 成年版毛片免费区| 91成年电影在线观看| 在线播放国产精品三级| 免费少妇av软件| 日本wwww免费看| 999精品在线视频| 交换朋友夫妻互换小说| 91九色精品人成在线观看| 日韩欧美在线二视频| 亚洲 国产 在线| 一区二区三区精品91| 97人妻天天添夜夜摸| 国产亚洲精品久久久久5区| 热re99久久国产66热| 国产精品九九99| 国产精品一区二区免费欧美| 午夜免费观看网址| 最近最新中文字幕大全电影3 | 成人永久免费在线观看视频| 交换朋友夫妻互换小说| 午夜激情av网站| 交换朋友夫妻互换小说| 免费日韩欧美在线观看| 国内毛片毛片毛片毛片毛片| 韩国av一区二区三区四区| 极品教师在线免费播放| 亚洲国产欧美网| 亚洲精品国产精品久久久不卡| 久久午夜综合久久蜜桃| 国产蜜桃级精品一区二区三区| 成人国语在线视频| 大型黄色视频在线免费观看| 久久香蕉激情| 身体一侧抽搐| 高清毛片免费观看视频网站 | 久久午夜综合久久蜜桃| 精品久久久久久,| 夜夜爽天天搞| 午夜日韩欧美国产| 欧美日韩中文字幕国产精品一区二区三区 | 亚洲少妇的诱惑av| 精品一区二区三区四区五区乱码| 国产又色又爽无遮挡免费看| 国产成年人精品一区二区 | 乱人伦中国视频| 久久草成人影院| 中文字幕人妻丝袜一区二区| 熟女少妇亚洲综合色aaa.| av视频免费观看在线观看| 中文字幕高清在线视频| av超薄肉色丝袜交足视频| 久久人人97超碰香蕉20202| 国产精品 欧美亚洲| 欧美日韩中文字幕国产精品一区二区三区 | 伦理电影免费视频| 免费高清在线观看日韩| 中文亚洲av片在线观看爽| 夜夜夜夜夜久久久久| 亚洲,欧美精品.| 国产亚洲精品综合一区在线观看 | 啪啪无遮挡十八禁网站| 欧美日韩瑟瑟在线播放| 久久人妻福利社区极品人妻图片| av国产精品久久久久影院| 午夜福利在线免费观看网站| 9191精品国产免费久久| 黄色视频,在线免费观看| 黑人巨大精品欧美一区二区mp4| 日本vs欧美在线观看视频| 国产精品免费一区二区三区在线| 黑人操中国人逼视频| 亚洲人成电影观看| 国产成人系列免费观看| 黄色丝袜av网址大全| 国产成年人精品一区二区 | 91精品三级在线观看| 免费在线观看日本一区| 啦啦啦 在线观看视频| 国产激情欧美一区二区| 亚洲国产精品一区二区三区在线| 国产高清视频在线播放一区| www.精华液| 嫩草影院精品99| 久久精品91蜜桃| 亚洲欧美精品综合久久99| 免费高清视频大片| 老司机在亚洲福利影院| 免费在线观看亚洲国产| 亚洲av美国av| 日韩精品中文字幕看吧| 午夜老司机福利片| 精品乱码久久久久久99久播| 在线十欧美十亚洲十日本专区| 在线观看免费午夜福利视频| 在线永久观看黄色视频| 久久精品亚洲精品国产色婷小说| 成年人黄色毛片网站| 日韩 欧美 亚洲 中文字幕| 99国产精品99久久久久| www.www免费av| 国产在线观看jvid| 久久国产亚洲av麻豆专区| www.www免费av| 成人三级黄色视频| 久久 成人 亚洲| www.www免费av| 国产在线观看jvid| 麻豆一二三区av精品| 十八禁人妻一区二区| 一级a爱片免费观看的视频| 啦啦啦在线免费观看视频4| 麻豆av在线久日| 成人三级黄色视频| 真人做人爱边吃奶动态| 男人的好看免费观看在线视频 | 人妻久久中文字幕网| 午夜福利免费观看在线| 久久精品91蜜桃| 亚洲精品国产一区二区精华液| 国产一区二区三区在线臀色熟女 | 精品久久久久久电影网| 国产精品二区激情视频| 欧美日韩精品网址| 亚洲成a人片在线一区二区| 日本黄色日本黄色录像| 侵犯人妻中文字幕一二三四区| 成年女人毛片免费观看观看9| 亚洲av日韩精品久久久久久密|