    Effects of sonication amplitude on the microstructure and mechanical properties of AZ91E magnesium alloy

    2023-01-08 10:22:02EmadiAndilabRavindran
    Journal of Magnesium and Alloys 2022年12期

    P.Emadi,B.Andilab,C.Ravindran

    Centre for Near-net-shape Processing of Materials,Ryerson University,350 Victoria Street,Toronto,ON M5B 2K3 Canada

    Abstract Light metals are gaining increased attention due to ecological sustainability concerns and strict emission regulations.Magnesium(Mg)is one such metal that has the potential to replace high density components,which can reduce emissions through lightweighting.However,the mechanical properties of Mg alloys must be improved for them to become viable candidates for structural applications.To this end,the current study examines the effect of sonication vibrational amplitude on the microstructure and mechanical properties of AZ91E Mg alloy.The molten alloys were subjected to ultrasonic treatment at a frequency of 20 kHz,180 s of processing time and vibrational amplitudes ranging from 1.25 to 15μm.The resultant castings were characterized using optical microscopy,scanning electron microscopy and tensile testing.It was found that sonication with amplitudes up to 7.5μm was able to effectively refin the secondary phases of the alloy.Similar trends were observed for grain size and yield strength.The refinemen in microstructure was likely caused by the fine grain size and cavitation induced undercooling of the liquid metal.In addition,it was also noted that even the lowest level of amplitude(1.25μm)was able to increase the density,improve the ultimate tensile strength and ductility of the castings.The tensile strength and ductility were thought to have been enhanced by ultrasonic degassing and refinemen in microstructure,while the yield strength was improved through the Hall-Petch effect.The results from this study provided a basis for optimizing the sonication process and promoting its use in industry.As a result,Mg alloys improved through ultrasonic processing have the potential to replace higher density components,with consequent energy efficien y and environmental and ecological benefits? 2022 Chongqing University.Publishing services provided by Elsevier B.V.on behalf of KeAi Communications Co.Ltd.This is an open access article under the CC BY-NC-ND license(http://creativecommons.org/licenses/by-nc-nd/4.0/)Peer review under responsibility of Chongqing University

    Keywords:Magnesium;Casting and solidification Ultrasonic processing;Vibrational amplitude;Grain refinement Mechanical properties.

    1.Introduction

    Magnesium(Mg)alloys are excellent candidates for replacing higher density metals such as iron(Fe)and aluminum(Al).Magnesium is abundant and possesses a high strengthto-weight ratio,making it a critical material where weight reduction is a priority[1,2].Lightweighting of electric vehicles,internal combustion vehicles and electronics is critical for emission reduction and ecological sustainability.Because of these factors,Mg has been gaining increasing attention throughout the past decades.The percentage of components made from Mg alloys is increasing year after year.However in order to further increase the use of Mg alloys in industry,there is a need to enhance its mechanical properties.

    Presently,most Mg alloys have poor tensile strength and ductility relative to Al alloys.Due to the low strength of Mg relative to other structural metals,its usage is limited to nonstructural components.Several methods have been proposed to improve the properties of cast Mg alloys.Some examples are The Elfina Process[3],Carbon inoculation[4]melt superheating[5]or sintering[6].Additionally,grain refinemen is also known to be a highly effective means for enhancing the strength of cast alloys[7,8].The grain refinemen process refers to the formation of fin grains which can improve strength and ductility through hindering dislocation motion at grain boundaries.Currently,zirconium(Zr)addition has been identifie as an effective means for the grain refinemen of Al-free Mg alloys[9].However,Zr addition is not effective for the more popular Al-bearing Mg alloys such as AZ91.This is in part due to reactions between Zr and Al available in the metal,which eliminates the grain refinin potential of Zr[2].

    The current methods for improving the properties of Mg alloys are inadequate.Zirconium addition fails to refin both Mg-Al and Al-free alloys and it is not cost effective.The Elfina process is only effective for Mg-Al alloys that contain manganese(Mn)and reduces alloy corrosion resistance due to Fe addition.Superheating is expensive,time consuming and increases the rate of oxidation as well as dissolved gasses.Carbon addition is mostly carried out through the addition of C2Cl6,but it leads to the emission of harmful gasses[10].As a result,an alternative method for the refinemen of Mg is required.Ideally,an effective refinin technique should be suitable for both Al-free and Al-bearing Mg alloys.

    Ultrasonic treatment(UST)has recently emerged as an effective means for the refinemen of metals and alloys[11-15].The process entails the application of high-intensity ultrasonic vibration to the liquid metal using a sonotrode.Sonication requires low-cost equipment and processing times are relatively short.Furthermore,it can be applied to both Al-free and Mg-Al alloys.However,the sonication process is poorly understood.Significan research and development are required in order to elevate the technology to a level for industrial application,especially for processing molten Mg alloys.

    While several studies in the fiel of ultrasonic processing of light metals are available,few have been completed with industrial application in mind[16].For example,a number of studies examine the effects of sonication during solidificatio[17-20].This is not effective for castings with complicated shapes since the sound waves cannot reach all areas of a complex mold.Other studies use lengthy refinin times,which is unacceptable from an efficien y perspective,since it leads to time lost during the casting process[21-23].In addition,several studies sonicate at high power levels,several times higher than the reported threshold for cavitation to occur[24-26].This leads to a higher level of energy consumption as well as more expensive equipment.Hence,further research is required to optimize sonication processing parameters,such as ultrasonic power,to improve its useability in industrial settings.

    The purpose of this research is to examine the effects of vibrational amplitude on the microstructure and mechanical properties of AZ91E Mg alloy,which was not extensively investigated in prior studies.Consequently,its effect on the properties and microstructure of Mg are not well understood.In this study the experimental procedure consisted of systematic increases in amplitude both above and below the threshold for cavitation to occur.This was done to clearly understand the impact of sonication amplitude on the resultant tensile properties and secondary phases of the alloy.The results from this study are critical for ultrasonic treatment process optimization in an industrial setting,especially since maintaining high levels of amplitude is more energy intensive.Therefore,Mg alloys improved through optimized sonication processes can lead to their increased use in the automotive,aerospace and electronics industries.

    Table 1Average chemical composition of AZ91E ingots.

    2.Materials and methods

    Ingots of AZ91E alloy with chemical composition detailed in Table 1 were used in this study.An electric resistance furnace was used for melting of the ingots.Prior to melting,the ingots were placed in a low-carbon steel crucible and preheated to 200 °C for 30 min.Subsequently,the ingots were heated to 740 °C for melting with an atmosphere of 4.7 L/min of CO2and 0.5 vol.% SF6to prevent oxidation.An ASTM standard B108-6 tensile mold was used[27].The mold was preheated to 350 °C prior to pouring to ensure adequate fillin and a controlled solidificatio rate.The liquid metal was poured at 720°C to match industrial practices.Two identical round tensile test coupons were produced from the same casting mold.

    Ultrasonic treatment was performed using a Sonic Systems UK ultrasonic vibration device(model L500).The frequency of vibration was fi ed at 20±1 kHz.The amplitude of vibration was varied from 1.25 to 15μm and applied to the liquid metal using a titanium alloy sonotrode.Sonication was carried out at a melt temperature of 740 °C for 180 s,with the sonotrode immersed 10 mm below the melt surface.After treatment,the surface of the liquid metal was skimmed of dross and poured.Two trials with a total of four samples per condition were evaluated to ensure repeatability of the results.

    Tensile testing was done using a United Universal Testing Machine(Model STM-50 kN)at a nominal pull rate of 12.5 mm/min.The %Elongation was measured with an extensometer attached to the gage section.Testing was done at ambient temperature.After testing was completed,sections for metallography were extracted 10 mm away from the fracture surface.Specimens were ground using SiC paper and polished using 9,3 and 1μm diamond compound with an ethanol-based dispersing agent.

    For grain size analysis,samples were solution heat treated at 413 °C for 24 hr,according to ASTM B661-12[28].To reveal the grain boundaries,the samples were etched using a 95% water and 5% citric acid solution,for 15 s with minor agitation.A Nikon Eclipse metallurgical microscope(Model MA200)was used to capture images for measuring grain size.For each sample,20 images were captured at 100X,and measurement was performed using Clemex Vision PE image analysis software with due consideration to ASTM E112-13[29].The microstructural analysis was carried out using a JEOL scanning electron microscope(SEM)(Model 6380LV),and the phases were identifie using EDX.

    Fig.1.Scanning electron micrographs of AZ91E sonicated with a vibrational amplitude of a)0μm(base alloy),b)1.25μm,c)3.75μm,d)7.5μm,e)11.25μm,and f)15μm.

    3.Results

    3.1.Microstructural analysis

    Fig.1a displays a backscattered electron micrograph of the base alloy.The microstructure consisted of theα-Mg matrix,β-Mg17Al12eutectic phase and Mn-Al intermetallics.In the base condition,massiveβ-Mg17Al12were observed,which precipitated in coarse networks.Theβ-phase is the last phase to form,so it typically precipitates from grain boundaries[30].The phase consists of three morphologies,lamellar,partially divorced and fully divorced.With the application of UST at 1.25μm,a noticeable change in the microstructure was not observed(Fig.1b).However,as observed in Fig.1c,increasing the amplitude to 3.75μm led to minor refinemen in theβ-phase.The previously massive networks appeared to be smaller in size and shorter in length.Further increasing the ultrasonic amplitude of vibration to 7.5μm,led to a marked refinemen in theβ-phase(Fig.1d).The massive eutectic morphology was completely absent,and the microstructure was dominated by short and fin networks.Moreover,the lamellar eutectics were more pronounced due to the absence of the largeβ-phase.Increasing the amplitude of vibration to 11.25 and 15μm did not appear to further enhance the eutectic phase(Fig.1e and f).

    In contrast to theβ-phase,the Mn-Al intermetallics are the firs phase to form during solidificatio[30].The intermetallics have been reported to act as nucleation sites forα-Mg[31].These phases usually present themselves in either needles or clusters of round particles,as observed in Fig.1a for the base condition.With the application of UST at 1.25μm,no change was observed in the shape and distribution of the Mn-Al phase(Fig.1b).However,as seen in Fig.1c,at a vibrational amplitude of 3.75μm,both the needle-like morphology and the clustering were not seen in the microstructure.Further increasing the amplitude to 7.5μm led to comparable results but with the phase appearing visually smaller(Fig.1d).No further changes were observed by increasing the amplitude beyond 7.5μm(Fig.1e and f).

    Fig.2.Optical micrographs of AZ91E sonicated with a vibrational amplitude of a)0μm(base alloy),b)1.25μm,c)3.75μm,d)7.5μm,e)11.25μm,and f)15μm.

    3.2.Grain size analysis and density

    Fig.2a displays an optical micrograph of the base alloy captured after solution heat treatment according to ASTM B661-12[28]and etching with citric acid.The microstructure of the base alloy primarily consisted of coarse grains with irregular grain boundaries.With the application of UST for 3 min at an amplitude of 1.25μm,a clear change in the microstructure was seen(Fig.2b).The grain boundaries became more regular,and the overall structure appeared to transition to a more equiaxed state.Moreover,a combination of smaller and larger grains was observed.A similar grain shape and size distribution was seen for the samples that underwent UST at 3.75μm vibrational amplitude,which can be seen in Fig.2c.However,upon increasing the amplitude of vibration to 7.5μm,the grain size was significantl fine compared to the base alloy,and the grain size distribution was more homogeneous(Fig.2d).Further increasing the vibrational amplitude to 11.25 and 15μm(Fig.2e and f)only serves to produce a more homogenous grain size distribution with no significan changes to the grain size.Effectively no change was observed by increasing the amplitude from 11.25 to 15μm.

    Fig.3.Average grain diameter of the AZ91E base alloy and the sonicated alloys,with error bars representing one standard deviation about the sample mean.

    The change in average grain size with varying UST vibrational amplitude can be seen in Fig.3.The grain size of the base alloy was 214±27μm.With the application of UST at 1.25μm amplitude,the grain size decreased to 145±30μm.Further increasing the vibrational amplitude to 3.75 decreased the grain size to 116±30μm.It must be noted that the error in average grain size was relatively high for the base alloy and the alloys processed at 1.25μm and 3.75μm amplitudes.This was due to the microstructure containing a combination of fin and coarse grains which was apparent in Fig.2a,b and c.The grain size of the alloy processed with a UST amplitude of 7.5μm was 73±7μm.The error in grain size at this level was smaller,which was in line with the optical microstructure observed in Fig.2d.The fines grain size,60±3μm,was observed for the samples that underwent UST at 11.25μm amplitude(72% decrease).Moreover,further increasing the amplitude to 15μm did not lead to a fine grain size.In effect,the grain sizes of the alloys processed 7.5,11.25 and 15μm amplitudes were similar.

    Fig.4.Density of the AZ91E base alloy and the sonicated alloys,with error bars representing one standard deviation about the sample mean.

    Fig.4 summarizes the density of the cast samples that was measured using the Archimedes principle.Measurements were taken from the same samples that were used for microstructure analysis.The density of the base alloy was measured as 1.785 g/cm3.This was significantl lower than the reported density of AZ91E,1.81 g/cm3[30].Such an outcome was expected since the casting procedure did not use a flu agent or degassing technique such as bubbling with inert gas.With the application of UST at 1.25μm amplitude,the density increased to 1.815 g/cm3.However,further increasing the vibrational amplitude did not appear to increase the density.Therefore,applying a range of vibrational amplitude from 1.25 to 15μm did not produce different outcomes.

    3.3.Mechanical properties

    The mechanical properties of the base and refine alloys measured by tensile testing at ambient temperature are summarized in Fig.5.The UTS of the base alloy was determined to be 138.7±1.9 MPa(Fig.5b).Upon applying ultrasonic treatment with a vibrational amplitude of 1.25μm,the UTS increased to 169.6±4.3 MPa.This translated to an increase in strength of approximately 22%.Further increasing the amplitude of vibration to 3.75,7.5,11.25 or 15μm did not improve the UTS.Fig.5c displays the ductility of the samples expressed as%Elongation(%EL).The ductility of the base alloy was 1.3±0.1%.After UST at 1.25μm amplitude,the%El increased to 3.0±0.3%(131%increase).Similar to the UTS,the ductility of the samples did not improve by increasing the vibrational amplitude beyond 1.25μm.

    For the base condition,the yield strength was 98.1±2.9 MPa.The YS improved with increasing vibrational amplitude up to 7.5μm.The YS for the 1.25μm vibrational amplitude was 99.6±0.1 MPa.Further increasing the amplitude to 3.75,increased the YS to 105.1±0.6%.The highest YS was achieved at the 7.5μm amplitude which was 110.0±1.2 MPa.In effect,the YS improved by approximately 12%.Increasing the amplitude to 11.25 or 15 did not further improve the YS.Upon examining Fig.5a,it is clear that the trend for YS differed from that of UTS and%EL.The tensile strength and ductility drastically improved with only 1.25μm vibrational amplitude and remained stable thereafter.In contrast,the yield strength of the alloys showed steady signs of improvement up to 7.5μm vibrational amplitude and did not increase for 11.25 and 15μm.

    Table 2Summary of parameters used for calculation of ultrasonic intensity.

    3.4.Ultrasonic intensity

    The Intensity of the sonication process is of critical importance during irradiation.It can be described as the ultrasonic energy that is transferred to the liquid metal through the sonotrode(Horn)[32].Sonication intensity(I)has been define by Eskin as[32]:

    Where,ρis the density of the liquid metal,c is the speed of sound in the liquid metal,fis the frequency of the sonication process and A is the vibrational amplitude.Quested et al.[33]reported the density of liquid AZ91 as 1.66 g/cm3.In our study,the frequency was 20 kHz and the vibrational amplitude ranged from 1.25 to 15μm.In an earlier study,the speed of sound in the liquid metal was set as 1500 m/s[34].It must be noted that the speed of sound in liquid AZ91E is not available in literature.As a result,researchers typically assume 1300 m/s as an approximation for low melting point metals[35].However,a logical assumption that has been utilized in past research is to assume the speed to be near that of the speed of sound in water at room temperature[34].Such an assumption is acceptable since liquid Mg has a density and viscosity that is near that of water.A summary of the parameters used is provide in Table 2.

    Using Eq.(1),the intensity of the sonication was plotted against the change in vibrational amplitude.The result is summarized in Fig.6.Researchers have reported that the minimum intensity needed to produce fully developed cavitation in Mg alloys is between 80 and 100 W/cm2[32,36].This level of intensity corresponds to amplitudes between 6.25 and 7.25μm.Furthermore,using vibrational amplitudes of 11.25 or 15μm would lead to intensities that are 2.4 and 4.2 times the minimum threshold for cavitation to occur,respectively.

    Fig.5.Tensile properties of the AZ91E base alloy and the sonicated alloys,a)%Elongation,b)Ultimate tensile strength and c)Yield strength,with error bars representing one standard deviation about the sample mean.

    Fig.6.Ultrasonic intensity calculated using Eq.(1).

    4.Discussion

    It was found that the base casting had a lower density compared to that of theoretical AZ91E alloy.That is,the density of the base casting was determined as 1.785 g/cm3while that of AZ91E is 1.81 g/cm3[30].It is likely that the lower density of the base casting was caused by porosity due to dissolved gasses.Especially,since no degassing agent was used as part of the experimental procedure.After the application of UST,the density of the samples was near that of the reported value for AZ91E.It must be noted that even sonicating with the minimum available amplitude of the system,1.25μm,led to an improvement in density.The improvement remained consistent with increasing vibrational amplitude up to 15μm.This result can be explained by the degassing ability of the sonication process.

    Research has shown that the cavitation process is highly effective in removing dissolved hydrogen from liquid metal[37,38].The degassing process operates through the accumulation of dissolved gas in pulsating bubbles through diffusion.This occurs during the rarefaction stage of bubble oscillation[32].Moreover,the cavitation bubbles then grow,coalesce to form larger bubbles,floa to the surface of the melt,and escape to the atmosphere.It should be mentioned that the effectiveness of ultrasonic degassing increases with the number of foreign particles or inclusions within the liquid metal[32].This is especially important for Mg alloys,since they have a high affinit for oxygen,which leads to the melt containing a large number of oxides relative to Al[39].With the considerable number of foreign particles in the melt,they act as substrates for the formation of cavitation bubbles,thereby effectively reducing the cavitation threshold[32].This can explain the outcome that even a small vibrational amplitude,far lower than the reported minimum needed for fully developed cavitation,can effectively degas the AZ91E alloy melt.

    Grain size reductions of up to 72% were achieved in this study.This was a result of UST at 11.25μm amplitude.However,it must be said that the range of amplitudes from 7.5 to 15μm produced comparable results.This is significan since the amplitude threshold for fully developed cavitation is approximately 7μm.As a result,once the cavitation is fully developed,increasing the amplitude of vibration any further will not lead to further improvements in grain size.

    The main mechanism of grain refinemen in this case was likely the wetting of fin oxides in the melt[40,41].The oxides in turn can act as heterogenous nucleation sites for the nucleation of Mg grains.This occurs through the cavitation phenomenon where the pulsating bubbles of gas undergo stages of expansion and compression until their eventual collapse[32].The collapse of gas bubbles can produce high intensity shock waves throughout the melt.The shockwaves have been reported to aid the liquid metal in reaching all areas of inclusions such as cracks and crevices that were previously fille with gas[32].It is likely that once cavitation is fully developed at approximately 7μm,a sufficien number of oxides are activated in the melt.It is known that only a fraction of nucleation sites or agents can contribute to the solidificatio process[42].As a result,although increasing the sonication intensity may in fact wet more inclusions,since only a fraction take part in solidification the newly activated substrates do not lead to a fine grain size.

    The secondary phases in this study were also considerably affected by the sonication process.The results showed that apart from the 1.25μm amplitude,all the sonicated alloys displayed signs of eutecticβ-Mg17Al12refinement In particular,with increasing sonication amplitude up to 7.5μm,theβ-phase became shorter in length and smaller in size.Such an outcome has been reported for grain refine castings of Mg[43].This is due to theβ-phase predominantly precipitating on grain boundaries.Moreover,since the grain size of the castings decreased with increasing amplitude,theβ-phase became more refined However,since the grain size did not change between 7.5 and 15μm,it would follow that theβphase would not be refine further.

    In addition to theβ-Mg17Al12phase,the Mn-Al based intermetallics were refine as well.In the base condition,the intermetallics were observed to be in either needle-like morphologies or clusters of round particles.However,as the sonication amplitude increased,both the shape and the distribution of the Mn-Al intermetallics were improved.Namely,the needle-like morphology was transformed to a more round shape.As well,the particle clustering was eliminated,and the phase became more evenly distributed throughout the Mg matrix.Such a transformation of the Mn-Al phase has been reported in the literature and is likely a result of the ultrasonic induced melt pressure changes[17,44].

    During the sonication process,if the intensity is sufficien to prompt cavitation,localized pressure changes can occur in the liquid metal.If the pressure change is high enough,certain areas in the melt can become undercooled,thereby triggering the formation of precipitates.This is especially important for the Mn-Al intermetallic,since it is the firs phase to form during solidification Alternatively,similar to theβphase,the refinemen of the Mn-Al phase was not observed after sonication with 1.25μm amplitude and only became apparent between 3.75μm and 15μm.This was to be expected since cavitation was likely not fully developed at lower amplitudes.As a result,the pressure changes would not have been sufficien to prompt nucleation.

    Both the tensile strength and the ductility of the castings showed improvements with the application of UST.It was observed that the improvements were similar for all UST amplitudes from 1.25 to 15μm.This was likely a result of the change in porosity of the castings.Porosity is known to have a detrimental effect on both UTS and ductility[45,46].Moreover,the trend observed for the change in density was almost identical to the changes in UST and ductility.This result suggested that the three parameters are likely linked.

    In contrast,the same trend as UTS and ductility was not observed for YS.This is likely due to the change in grain size of the alloys with UST.According to the classical Hall-Petch relation,the YS of metals and alloys typically improve with decreasing grain size.In this study,the grain size of the alloys decreased with increasing vibrational amplitude up to 7.5μm and was stable thereafter.Similarly,the YS of the casting followed the same trend.

    The refinemen of secondary phases would also have a positive influenc on the tensile properties of the sonicated alloys.As mentioned previously,theβ-Mg17Al12eutectic phase predominantly precipitates on grain boundaries in the form of continuous networks.The phase is deleterious to mechanical properties due to its brittle nature[30].Therefore,refinemen of theβ-phase would likely bring about noticeable improvements in mechanical properties.In addition,refine ment of the Mn-Al phase likely contributed to improving mechanical properties as well.As observed in a previous study,spheroidization of these brittle phases and their homogenous distribution can reduce stress concentrations in the microstructure and prevent premature failure of the castings[13].

    It is clear ultrasonic treatment is an effective method to improve the microstructure and mechanical properties of permanent mold cast AZ91E alloy.Even a minor vibrational amplitude was shown to improve the UTS,YS,ductility,and density of the castings.However,higher amplitudes up to 7.5μm were required to produce optimal grain size and YS.It was also observed that once the cavitation was theoretically determined to be fully developed at 7.5μm,increasing the vibrational amplitude had little to no effect on the resultant mechanical properties and microstructural features.Ultrasonic treatment is significan in its capacity to refin cast alloys,since it can do so without altering the chemistry of the alloy.This is critical since in many applications chemical compositions cannot be altered.

    This study presents an important analysis pertaining to the effects of vibrational amplitude on the effectiveness of UST,which can provide a step towards improving the sonication process and promoting its industrial application.It must be noted that future work is required to fully optimize UST.In particular,the effects of varying sonication time at different vibrational amplitudes as well as the role of sonotrode depth must be investigated.As a result,cast Mg alloys refine with UST have the potential to replace high density Al and Fe based alloys,leading to lightweighting and improved efficien y.

    5.Conclusion

    This study examined the effects of UST on the microstructure and mechanical properties of AZ91E Mg alloy.Permanent mold cast samples were prepared using a fi ed sonication frequency and sonotrode depth with vibrational amplitudes varying from 2.5 to 15μm.The castings were evaluated based on grain size,secondary phase characteristics and tensile properties.Small vibrational amplitudes resulted in significan changes to grain size and secondary phases.Similar trends were seen for the strength properties and the density.The results of this study enabled a comprehensive understanding of the relationships between microstructural features,mechanical properties,and UST vibrational amplitude.

    The following conclusions can be drawn from this study:

    1 Ultrasonic treatment led to the refinemen of the alloy grain size.Specificall,the grain size decreased steadily up to 7.5μm vibrational amplitude but,only slight changes were observed by increasing the amplitude to 11.25 and 15μm.It was suggested that the grain size was enhanced through heterogenous nucleation from newly wetted fin oxides present in the liquid metal.

    2 A similar trend was observed for secondary phases.Gradual improvements were observed up to 7.5μm vibrational amplitude with no change thereafter.The refinemen inβ-Mg17Al12phase was thought to be a result of the change in grain size.Alternatively,the change in Mn-Al intermetallics were suggested to have been caused by cavitation induced undercooling of the liquid metal.

    3 The YS of the samples also increased up to 7.5μm amplitude and remained stable thereafter.The increase in YS was thought to be a result of fine grain size through Hall-Petch strengthening.

    4 The density of the sonicated castings showed a sudden improvement with application of UST at 1.25μm amplitude.Increasing the amplitude up to 15μm did not change the density further.The change in density was suggested to have occurred through ultrasonic degassing of the melt.

    5 The UTS and ductility also improved with the application of 1.25μm vibrational amplitude with no changes thereafter.This was thought to be a result of the change in density due to sonication,which followed an identical trend.

    Declaration of Competing Interest

    None.

    Acknowledgements

    The authors recognize the kind support of the Natural Sciences and Engineering Research Council(NSERC)for the award of Canada Graduate Scholarships(CGSD3-535728-2019 and CGSD3-559982-2021).The authors would like to thank Mr.Alan Machin and Mr.Adam Belcastro for their support with this research.

    久久人妻av系列| 欧美黑人巨大hd| 老汉色av国产亚洲站长工具| 精品乱码久久久久久99久播| 国产免费av片在线观看野外av| 国产蜜桃级精品一区二区三区| 欧美又色又爽又黄视频| 日本免费一区二区三区高清不卡| 亚洲国产看品久久| 免费高清视频大片| 淫秽高清视频在线观看| 国产亚洲欧美在线一区二区| 黄色女人牲交| 国产精品av视频在线免费观看| 美女黄网站色视频| 五月玫瑰六月丁香| 88av欧美| 1024香蕉在线观看| 国产精品久久久久久精品电影| 一进一出好大好爽视频| www日本黄色视频网| 国产精品影院久久| 亚洲av成人不卡在线观看播放网| 在线观看www视频免费| 久久精品91蜜桃| 欧美日韩黄片免| 身体一侧抽搐| 亚洲一区二区三区色噜噜| 精品国产超薄肉色丝袜足j| 国产一级毛片七仙女欲春2| 好男人电影高清在线观看| 天天躁夜夜躁狠狠躁躁| 久久欧美精品欧美久久欧美| 国产精品亚洲一级av第二区| 精品不卡国产一区二区三区| 亚洲成人免费电影在线观看| 国产午夜福利久久久久久| 精品国产亚洲在线| 每晚都被弄得嗷嗷叫到高潮| 成人国产综合亚洲| 国产精品免费视频内射| 亚洲熟女毛片儿| 999精品在线视频| 国产99白浆流出| 久久久久久免费高清国产稀缺| 悠悠久久av| 国产精品久久久久久亚洲av鲁大| 色在线成人网| 欧美在线黄色| 色噜噜av男人的天堂激情| 久久天堂一区二区三区四区| 亚洲精品美女久久久久99蜜臀| 国产精品九九99| 亚洲九九香蕉| 一个人免费在线观看的高清视频| 亚洲av熟女| 俄罗斯特黄特色一大片| 久久久久久国产a免费观看| 香蕉丝袜av| 久久天躁狠狠躁夜夜2o2o| 99在线视频只有这里精品首页| 久久久久久亚洲精品国产蜜桃av| 欧美日韩亚洲国产一区二区在线观看| 久久国产精品人妻蜜桃| 中文字幕高清在线视频| 亚洲最大成人中文| 精品一区二区三区视频在线观看免费| 老熟妇仑乱视频hdxx| 午夜免费成人在线视频| 亚洲自拍偷在线| 伊人久久大香线蕉亚洲五| 国产亚洲精品第一综合不卡| 国产主播在线观看一区二区| 国产又色又爽无遮挡免费看| 国内揄拍国产精品人妻在线| www日本黄色视频网| 亚洲成人国产一区在线观看| 黄色视频不卡| 成在线人永久免费视频| 99久久无色码亚洲精品果冻| 久久久国产成人免费| 久久久久性生活片| 国产v大片淫在线免费观看| 精品乱码久久久久久99久播| 琪琪午夜伦伦电影理论片6080| 国产成人精品无人区| 国产精品 国内视频| 国产成人精品无人区| 成年人黄色毛片网站| av片东京热男人的天堂| 熟女少妇亚洲综合色aaa.| 久久人妻av系列| 午夜日韩欧美国产| 成年版毛片免费区| 丰满人妻熟妇乱又伦精品不卡| 亚洲在线自拍视频| 国产亚洲精品一区二区www| 一级黄色大片毛片| 日本免费一区二区三区高清不卡| 亚洲国产高清在线一区二区三| netflix在线观看网站| 99久久综合精品五月天人人| 18禁裸乳无遮挡免费网站照片| 女生性感内裤真人,穿戴方法视频| 99re在线观看精品视频| 欧美三级亚洲精品| 日韩欧美在线乱码| 蜜桃久久精品国产亚洲av| a级毛片在线看网站| 哪里可以看免费的av片| 一a级毛片在线观看| 曰老女人黄片| 脱女人内裤的视频| 欧美极品一区二区三区四区| 男人的好看免费观看在线视频 | 又紧又爽又黄一区二区| 看黄色毛片网站| 亚洲欧洲精品一区二区精品久久久| 欧美色视频一区免费| 大型av网站在线播放| av有码第一页| 成在线人永久免费视频| 一级片免费观看大全| 久久久精品国产亚洲av高清涩受| 久久伊人香网站| 啦啦啦观看免费观看视频高清| 特级一级黄色大片| 国产精品1区2区在线观看.| 黄色 视频免费看| 亚洲国产精品999在线| 亚洲av美国av| 99在线人妻在线中文字幕| 两个人视频免费观看高清| 亚洲精品久久国产高清桃花| 美女 人体艺术 gogo| 亚洲第一电影网av| 亚洲av成人一区二区三| 麻豆成人av在线观看| 午夜福利在线在线| 国产91精品成人一区二区三区| 国产一区二区三区在线臀色熟女| 亚洲精品中文字幕一二三四区| 午夜精品在线福利| 欧美一级毛片孕妇| 黄色a级毛片大全视频| 9191精品国产免费久久| 熟妇人妻久久中文字幕3abv| 妹子高潮喷水视频| 国产成人系列免费观看| 亚洲精品美女久久av网站| 我要搜黄色片| 国产av又大| 国产精品亚洲av一区麻豆| 高潮久久久久久久久久久不卡| 亚洲欧美日韩东京热| 久久久久久人人人人人| 日本 av在线| 欧美一区二区国产精品久久精品 | 性欧美人与动物交配| 正在播放国产对白刺激| 国产伦在线观看视频一区| 久久久久久人人人人人| 日韩欧美一区二区三区在线观看| 琪琪午夜伦伦电影理论片6080| av视频在线观看入口| 久99久视频精品免费| 99热这里只有精品一区 | 狠狠狠狠99中文字幕| 欧美成狂野欧美在线观看| 免费看日本二区| 久久午夜综合久久蜜桃| 亚洲av片天天在线观看| 婷婷精品国产亚洲av| 最好的美女福利视频网| 久久中文看片网| 两个人视频免费观看高清| 黄色片一级片一级黄色片| 午夜精品一区二区三区免费看| 国内精品一区二区在线观看| 三级国产精品欧美在线观看 | www日本黄色视频网| 精品乱码久久久久久99久播| 免费搜索国产男女视频| 国产亚洲欧美98| 亚洲 欧美一区二区三区| 国产成+人综合+亚洲专区| 嫩草影视91久久| 亚洲av免费在线观看| 国产一区二区在线av高清观看| 亚洲高清免费不卡视频| 国产69精品久久久久777片| 天堂网av新在线| 国产黄片美女视频| 国产精品久久久久久亚洲av鲁大| 热99在线观看视频| 日本爱情动作片www.在线观看| 欧美日韩精品成人综合77777| 亚洲无线在线观看| 禁无遮挡网站| 校园春色视频在线观看| 91精品一卡2卡3卡4卡| 97超碰精品成人国产| 日本成人三级电影网站| 自拍偷自拍亚洲精品老妇| 99在线人妻在线中文字幕| 久久国内精品自在自线图片| 久久久久久久久久久丰满| 看十八女毛片水多多多| 精品久久久久久久久亚洲| 久久久精品欧美日韩精品| 亚洲四区av| 直男gayav资源| 成人永久免费在线观看视频| 亚洲成人久久性| 色综合亚洲欧美另类图片| 亚洲aⅴ乱码一区二区在线播放| 麻豆乱淫一区二区| 国产色爽女视频免费观看| 少妇高潮的动态图| 少妇人妻一区二区三区视频| 淫秽高清视频在线观看| 日本欧美国产在线视频| 又爽又黄a免费视频| 成年版毛片免费区| 精品久久久久久久久亚洲| 噜噜噜噜噜久久久久久91| 日韩亚洲欧美综合| 久久人妻av系列| 久久久久久久久久久免费av| 久久99蜜桃精品久久| 亚洲精品国产成人久久av| 99久久精品国产国产毛片| 99久久人妻综合| 成年版毛片免费区| av天堂在线播放| 国产一区亚洲一区在线观看| 六月丁香七月| 国产91av在线免费观看| 国产亚洲精品av在线| 全区人妻精品视频| 久久精品91蜜桃| 亚洲精品亚洲一区二区| 久久久午夜欧美精品| 此物有八面人人有两片| 神马国产精品三级电影在线观看| 日韩精品青青久久久久久| 日本五十路高清| 天天躁夜夜躁狠狠久久av| 成人毛片60女人毛片免费| 一区二区三区高清视频在线| 国内少妇人妻偷人精品xxx网站| 两个人的视频大全免费| 1000部很黄的大片| 只有这里有精品99| 深夜a级毛片| 日韩中字成人| 国产精品av视频在线免费观看| 国产精品久久久久久精品电影| 国产精品,欧美在线| 亚洲精品粉嫩美女一区| 亚洲av免费高清在线观看| 丝袜喷水一区| av.在线天堂| 亚洲av成人av| 男插女下体视频免费在线播放| 亚洲图色成人| 国产高清不卡午夜福利| 久久99热这里只有精品18| 亚洲精品影视一区二区三区av| 国产精品久久电影中文字幕| 白带黄色成豆腐渣| av免费观看日本| 欧美zozozo另类| 欧美极品一区二区三区四区| 日韩成人伦理影院| 男人舔奶头视频| 我要搜黄色片| 女人被狂操c到高潮| 国产精品人妻久久久久久| 神马国产精品三级电影在线观看| 中文字幕熟女人妻在线| 亚洲成人久久爱视频| 午夜精品一区二区三区免费看| 91久久精品电影网| 亚洲内射少妇av| 18禁在线无遮挡免费观看视频| 久久久a久久爽久久v久久| 永久网站在线| 国产成人福利小说| 亚洲高清免费不卡视频| 国产亚洲av片在线观看秒播厂 | 色噜噜av男人的天堂激情| 午夜福利在线观看吧| 久久久a久久爽久久v久久| av专区在线播放| 国产极品天堂在线| 综合色丁香网| 老司机福利观看| 夫妻性生交免费视频一级片| 久久久久久伊人网av| 日韩欧美精品免费久久| 亚洲欧美日韩高清在线视频| 欧美色欧美亚洲另类二区| 男女视频在线观看网站免费| 午夜福利视频1000在线观看| 少妇人妻精品综合一区二区 | 亚洲国产精品国产精品| 国产高清三级在线| 欧美高清成人免费视频www| 国产精品乱码一区二三区的特点| 亚洲精品亚洲一区二区| 亚洲成人精品中文字幕电影| 国产精品久久久久久精品电影| 国产国拍精品亚洲av在线观看| 免费大片18禁| 久久九九热精品免费| 干丝袜人妻中文字幕| 国产午夜精品一二区理论片| 亚洲中文字幕日韩| 成人三级黄色视频| or卡值多少钱| 能在线免费看毛片的网站| 国产麻豆成人av免费视频| 老司机福利观看| 欧美一级a爱片免费观看看| 国产精品不卡视频一区二区| 22中文网久久字幕| 日韩强制内射视频| 男人狂女人下面高潮的视频| 欧美激情久久久久久爽电影| 久久精品国产亚洲av香蕉五月| 天天躁日日操中文字幕| 天堂网av新在线| 国产乱人视频| 欧美日韩乱码在线| 九九爱精品视频在线观看| 人体艺术视频欧美日本| 国产亚洲91精品色在线| 美女 人体艺术 gogo| 国产午夜精品论理片| 男人舔女人下体高潮全视频| 在线观看午夜福利视频| 青春草视频在线免费观看| 天天躁夜夜躁狠狠久久av| 欧美一区二区亚洲| 国产乱人偷精品视频| 三级男女做爰猛烈吃奶摸视频| 亚洲熟妇中文字幕五十中出| 99热6这里只有精品| 久久鲁丝午夜福利片| 国产精品久久久久久精品电影| av女优亚洲男人天堂| 久久精品国产亚洲av涩爱 | 免费看av在线观看网站| 午夜精品一区二区三区免费看| 又爽又黄a免费视频| 国产极品天堂在线| 51国产日韩欧美| 国产蜜桃级精品一区二区三区| 成年版毛片免费区| 成年版毛片免费区| 久久欧美精品欧美久久欧美| 激情 狠狠 欧美| 人妻久久中文字幕网| 夫妻性生交免费视频一级片| 亚洲国产欧美人成| 老司机福利观看| 国产女主播在线喷水免费视频网站 | 身体一侧抽搐| 国产一区二区亚洲精品在线观看| 久久久国产成人精品二区| 精品不卡国产一区二区三区| 国产一区二区亚洲精品在线观看| 内地一区二区视频在线| 国产免费一级a男人的天堂| 变态另类丝袜制服| 晚上一个人看的免费电影| 精品熟女少妇av免费看| 国产精品女同一区二区软件| 又爽又黄a免费视频| 人妻夜夜爽99麻豆av| 亚洲七黄色美女视频| 日韩大尺度精品在线看网址| 亚洲激情五月婷婷啪啪| 夜夜爽天天搞| 精品久久久久久久人妻蜜臀av| 久久亚洲精品不卡| 久99久视频精品免费| 看十八女毛片水多多多| 波多野结衣高清作品| 国产单亲对白刺激| 欧美日韩综合久久久久久| 九九热线精品视视频播放| 亚洲欧美精品综合久久99| 国产高潮美女av| 狠狠狠狠99中文字幕| 日韩欧美国产在线观看| 天天躁夜夜躁狠狠久久av| 91久久精品国产一区二区成人| av专区在线播放| 精品一区二区免费观看| 最近的中文字幕免费完整| 在线观看66精品国产| 久久精品夜夜夜夜夜久久蜜豆| 久久久久久久午夜电影| 99riav亚洲国产免费| 成年av动漫网址| 国产免费男女视频| 日韩精品青青久久久久久| 精品午夜福利在线看| 男人的好看免费观看在线视频| 欧美极品一区二区三区四区| 真实男女啪啪啪动态图| 欧美日韩国产亚洲二区| 91午夜精品亚洲一区二区三区| 床上黄色一级片| 欧美xxxx性猛交bbbb| 亚洲欧美日韩高清在线视频| 不卡一级毛片| 亚洲18禁久久av| 免费在线观看成人毛片| av.在线天堂| 69av精品久久久久久| 精品久久久噜噜| 少妇丰满av| 久久久久性生活片| 欧美三级亚洲精品| 69人妻影院| 亚洲av中文字字幕乱码综合| 国产一区二区在线观看日韩| 亚洲成人久久爱视频| 色综合色国产| 中国国产av一级| 黄色欧美视频在线观看| 黄片wwwwww| 久久精品久久久久久久性| 亚洲电影在线观看av| 欧美性猛交╳xxx乱大交人| 亚洲天堂国产精品一区在线| 日本五十路高清| 国内精品宾馆在线| 看十八女毛片水多多多| 丰满乱子伦码专区| 亚洲av成人精品一区久久| 3wmmmm亚洲av在线观看| 国产精品久久久久久精品电影小说 | 国产精品一区二区三区四区久久| 国内久久婷婷六月综合欲色啪| 蜜臀久久99精品久久宅男| 久久午夜福利片| 国产成人一区二区在线| 国产亚洲91精品色在线| 老司机福利观看| 日本免费一区二区三区高清不卡| 欧美zozozo另类| 欧美变态另类bdsm刘玥| 免费av毛片视频| 日本三级黄在线观看| 日韩欧美精品v在线| 久久久久久久久大av| 91精品国产九色| 麻豆久久精品国产亚洲av| 99久久无色码亚洲精品果冻| 国产精品人妻久久久久久| 长腿黑丝高跟| 欧洲精品卡2卡3卡4卡5卡区| 国产三级在线视频| 简卡轻食公司| 波野结衣二区三区在线| 免费观看人在逋| 麻豆一二三区av精品| 99久久中文字幕三级久久日本| 婷婷色av中文字幕| 男女啪啪激烈高潮av片| 麻豆国产av国片精品| 国语自产精品视频在线第100页| 亚洲最大成人av| 大又大粗又爽又黄少妇毛片口| 色噜噜av男人的天堂激情| 久久人人爽人人片av| 美女脱内裤让男人舔精品视频 | 亚洲精品456在线播放app| 精品熟女少妇av免费看| 亚洲国产精品成人综合色| 91狼人影院| 青春草亚洲视频在线观看| 日韩一区二区视频免费看| 国产精品国产三级国产av玫瑰| 亚洲不卡免费看| 婷婷色综合大香蕉| 夜夜夜夜夜久久久久| 亚洲精品乱码久久久久久按摩| 久久久久网色| av.在线天堂| 一个人观看的视频www高清免费观看| 国产伦在线观看视频一区| 床上黄色一级片| 国产色婷婷99| 久久精品国产亚洲av香蕉五月| 极品教师在线视频| 日产精品乱码卡一卡2卡三| 国产成人aa在线观看| av在线蜜桃| 性色avwww在线观看| .国产精品久久| 99国产精品一区二区蜜桃av| 国产成人freesex在线| 偷拍熟女少妇极品色| kizo精华| 国产成人福利小说| 久久久精品大字幕| 黑人高潮一二区| 一本精品99久久精品77| 欧美bdsm另类| 成年av动漫网址| 18禁黄网站禁片免费观看直播| 女人被狂操c到高潮| 日日啪夜夜撸| 99热6这里只有精品| 日韩精品青青久久久久久| 国产精品美女特级片免费视频播放器| 永久网站在线| 最近手机中文字幕大全| 免费无遮挡裸体视频| 一边亲一边摸免费视频| 国产探花在线观看一区二区| 免费电影在线观看免费观看| 国产在视频线在精品| 男人舔女人下体高潮全视频| 中文字幕免费在线视频6| 亚洲欧美日韩无卡精品| 男人狂女人下面高潮的视频| 少妇人妻一区二区三区视频| 久久草成人影院| 久久精品久久久久久噜噜老黄 | 国产精品永久免费网站| 搡女人真爽免费视频火全软件| 别揉我奶头 嗯啊视频| 一区福利在线观看| 九九爱精品视频在线观看| 国产高清激情床上av| 亚洲不卡免费看| 亚洲美女视频黄频| 又爽又黄a免费视频| 国产精品免费一区二区三区在线| 一本精品99久久精品77| 国产精品一及| 又黄又爽又刺激的免费视频.| 五月玫瑰六月丁香| 国产成人a区在线观看| 免费观看a级毛片全部| 久久草成人影院| 黄片wwwwww| 欧美高清性xxxxhd video| 久久精品夜夜夜夜夜久久蜜豆| 99热这里只有精品一区| eeuss影院久久| 精品久久久久久成人av| 午夜福利在线在线| 日本一二三区视频观看| 免费av不卡在线播放| 成人无遮挡网站| 一级黄色大片毛片| 精品免费久久久久久久清纯| 少妇的逼水好多| 色吧在线观看| 别揉我奶头 嗯啊视频| 国产私拍福利视频在线观看| 国产大屁股一区二区在线视频| 丰满人妻一区二区三区视频av| 久久人妻av系列| 变态另类丝袜制服| 国产精品野战在线观看| 国产精品日韩av在线免费观看| 看片在线看免费视频| 中国国产av一级| 精品少妇黑人巨大在线播放 | 嫩草影院入口| 欧美最新免费一区二区三区| 亚洲婷婷狠狠爱综合网| 国产精品久久久久久久电影| 好男人在线观看高清免费视频| 日本免费一区二区三区高清不卡| 少妇人妻精品综合一区二区 | 搡老妇女老女人老熟妇| 成年版毛片免费区| 99riav亚洲国产免费| 亚洲国产高清在线一区二区三| 久久午夜亚洲精品久久| 天堂中文最新版在线下载 | 亚洲婷婷狠狠爱综合网| 插逼视频在线观看| 老司机影院成人| 此物有八面人人有两片| 久久精品久久久久久久性| 久久精品国产自在天天线| 国产av一区在线观看免费| av又黄又爽大尺度在线免费看 | 久久精品国产亚洲网站| 久久99精品国语久久久| 亚洲精品456在线播放app| 99久久精品热视频| 亚洲人成网站高清观看| 国产精品三级大全| 国产成人freesex在线| 一边摸一边抽搐一进一小说| 91久久精品电影网| 啦啦啦啦在线视频资源| av免费观看日本| 日韩欧美国产在线观看| 国产黄a三级三级三级人| 在线播放无遮挡| 久久6这里有精品| 在线观看免费视频日本深夜| 男插女下体视频免费在线播放|