    Research on the Pitting Mechanism of Dispersion-Strengthened High-Strength Steel Under Wet-Dry Cycling in a Marine Environment

    2021-12-22 11:40:24LIPingGENGYanmingandDUMin
    Journal of Ocean University of China 2021年6期

    LI Ping, GENG Yanming, and DU Min

    Research on the Pitting Mechanism of Dispersion-Strengthened High-Strength Steel Under Wet-Dry Cycling in a Marine Environment

    LI Ping, GENG Yanming, and DU Min*

    The Key Laboratory of Marine Chemistry Theory and Technology, Ministry of Education, College of Chemistry and Chemical Engineering, Ocean University of China, Qingdao 266100, China

    Due to the wet-dry cycling in the ocean tidal zone, the supply of dissolved oxygen and salt-containing particles were sufficient, so the corrosion was serious. Pitting corrosion was a common form of localized corrosion. This paper studied the pitting corrosion mechanism of dispersion-strengthened high-strength steel under different wet-dry ratio environments. Electrochemical Impedance Spectroscopy was used to study the changes of corrosion rate and electric double layer structure of the dispersion- strengthened high-strength steel. Scanning electron microscope, Raman spectroscopy, electron probe microanalysis and laser confocal scanning microscope were used to observe the corrosion product morphologies, analyze the corrosion product compositions, analyze the secondary distribution of alloy elements in the corrosion products and analyze the pitting information of the steel after the corrosion products were removed. The results showed that the degree of the steel corrosion was slight when the wetting time was longer, the size and depth of the corrosion pits on the surface were smaller. This was because the environment with longer wetting time made the corrosion products denser. In this environment, the conversion of γ-FeOOH to Fe3O4was promoted. In addition, it could also promote the alloying elements to be more concentrated in the rust layer. The above phenomena hindered the further corrosion of the matrix by dissolved oxygen and Cl?in the seawater.

    marine; dispersion-strengthened high-strength steel; wet-dry cycling; pitting; rust

    1 Introduction

    The ocean tidal zone had sufficient supply of dissolved oxygen and salt-containing particles due to the wet-dry cycling conditions. Therefore, the corrosion rate of marine steel structures in the tidal zone was greater than that in the seawater full immersion zone. Generally, the average corrosion rate in the tidal zone of the spray was 0.3–0.5mmyr?1, and the local corrosion were relatively more serious (Yu., 2018). Pitting corrosion was one of the most common forms of local corrosion in marine atmospheric environment (Park., 2015; Wang., 2015). In the drying stage of wet-dry cycling environment, with the decrease of humidity, Cl?in the liquid film was concentrated. When Cl?exceeded the critical concentration, pitting would occur on the surface of high-strength steel. Pitting corrosion was difficult to detect at the beginning of its occurrence. The pitting corrosion that occurred in the equipment could cause perforation of steel materials, which greatly brings about the construction safety hazards and economic losses. The rust layer form- ed on the surface of steel structure was also very important for corrosion in the marine tidal zone (Evans and Taylor, 1972; Stratmann., 1989). Due to the sufficient supply of dissolved oxygen during the dry wet alternation process, the oxidizing effect of the rust layer itself increased the cathodic current, and the nature of the rust layer would affect the pitting corrosion of steel (Wang., 2019; Zhang and Ma, 2019).

    There were many factors that affected the induction of pitting corrosion, such as inclusions, alloy elements, rust layers and so on (Soltis, 2015). This paper studied a new type of high-strength steel that was dispersion-streng- thened (a strengthening method by adding hard particles to a homogeneous material). Shi. (2019) used transmission electron microscope, high resolution transmission electron microscope, three-dimensional atom probe, ato- mic force microscope and combined with first-principles calculation method to study the dispersion-strengthened high-strengthened steel nano-precipitated phase. The experimental results showed that a large number of dispersed nano-precipitates were distributed in the matrix of dispersion-strengthened high-strength steel. Its size was a few nanometers to tens of nanometers and the main components were C, N, Ti, Nb, V,. Its crystal structure was FCC face centered cubic structure. The pitting corrosion resistance of this high-strength steel is not yet known. This kind of steel added a variety of corrosion-resistant alloying elements Cr, Ni, Mo,., as shown in Table 1. The relationship between the corrosion resistance of steel structure materials and alloying elements in marine environments varied with the environment (Díaz., 2018). The alloying elements in low-alloy steel have a certain impact on the corrosion resistance of steel structures in the marine tidal zone. The influence of the same alloying elements on steel structures (such as steel pile wharves, offshore oil platforms,.) starting from the marine atmosphere zone, passing through the marine wave splash zone, the marine tidal range, the seawater full immersion zone and the submarine mud zone were also completely different (Nishimura., 2001). Chen (2005) believed that certain alloying elements could improve the corrosion resistance of steel materials in the marine tidal zone, but the effect on the seawater full immersion area was not obvious, and may increase the corrosion rate.

    In this paper, the influence of different dry and wet ratios on the rust layer was studied by simulating the wet- dry cycling environment of the marine. And from the per- spective of the rust layer, the pitting mechanism of the dispersion-strengthened high-strength steel was discuss- ed.

    2 Experiment

    2.1 Experimental Materials and Medium

    The research object was dispersion-strengthened high- strength steel, and its chemical composition was shown in Table 1. The steel samples were cut into 10mm×10 mm×3mm and polished with 800#, 1000# and 2000# water matte paper in order to light. Wash the surface with distilled water and absolute ethanol respectively.

    The experimental medium was the natural seawater of Qingdao Wheat Island.

    Table 1 Compositions of dispersion-strengthened high-strength steel

    2.2 Wet-Dry Cycling Settings

    The pitting corrosion behavior of steel under two different dry wet cycles was studied. Taking 12h as a cycle period, one was drying for 10h and wetting for 2h, the other was drying for 2h and wetting for 10h. The dry-wet ratios were 5:1 and 1:5 respectively. Hang the samples in the experiment box with a glass rod, so that the samples were in a wet-dry cycling environment (Table 2).

    Table 2 Schedule of dry and wet cycles

    2.3 Experimental Methods

    Electrochemical impedance spectroscopy (EIS) tests were carried out in a three-electrode cell through a Germany Reference 600 electrochemical measurement system. Dispersion-strengthened high-strength steel was a working electrode that was embedded in an epoxy resin PVC holder in a square form (10mm×10mm×3mm) with a working area of 1cm2. A platinum electrode and a saturated calomel electrode (SCE) were used, respectively, as auxiliary and reference electrodes. Before the electrochemical test, took the electrode out of the experimental device and put it in a jar filled with seawater and let it stand for 30min to stabilize the open circuit potential (OCP) of the steel. The test frequency range was 100kHz –10mHz, and the amplitude of the sine wave AC signal was 10mV with respect to OCP.

    JSM-6700F scanning electron microscope (SEM) was used to observe the morphology of the inner and outer rust layers of dispersion-strengthened high-strength steel.

    Raman spectroscopy was used to determine the compositions of the rust layers. A DXR Microscope model of Raman spectrometer was used, the selected light source was 532nm, and the scanning range was 0–1500cm?1.

    JXA-8230 electron probe microanalysis (EPMA) was used to test the distribution of alloying elements in the rust layer. First took the sample out of the experimental device and rinsed it with distilled water. After it dries, it was sealed with epoxy resin. The section of the rust layer was exposed, and then polished to smooth with 800# and 1000# water matte paper respectively. Then put it into the electron probe microanalyzer, and selected a rectangular area containing the inner and outer rust layers, and detected the element distribution in this area.

    VK-X200 laser confocal scanning microscope (LCSM) was used to observe the pitting on sample surface after removing corrosion products. In each test, four different areas on the same straight line were selected for observation. After obtaining the pitting corrosion data, used data analysis software to build a 3D model for analysis. The pitting corrosion information listed in this paper were the average of 4 data in this environment.

    3 Results and Discussion

    3.1 Electrochemical Analysis

    Fig.1 was the EIS plots of the dispersion-strengthened high-strength steel under two dry and wet environments. When the drying time was longer (cycle I), it could be seen in the Nyquist plot (Fig.1(a)) that it was composed of a single capacitive loop during the first 5d of corrosion. After 10d of corrosion, it consisted of a semicircle in the high frequency area and a diagonal line in the low frequency area. The diagonal line in the low frequency area indicated the presence of Warburg. Warburg was related to the propagation and diffusion process of materials near the interface. This indicated that the corrosion products generated on the electrode surface at this time had an impact on the electrochemical process. At this time, the elec- trochemical process on the electrode surface was controlled by the mixing of the charge transfer process and the diffusion process. However, when the wetting time was longer (cycle II), the Warburg did not appear until 30d after corrosion.

    The modulus of the impedance in the intermediate frequency zone had a linear relationship with frequency and both were less than ?1. When the slope was close to ?1, the surface state of the electrode was completer and more compact. It meant that the electrode was closer to the complete capacitor (Porcayo., 2017). After the same corrosion time, the slope of the intermediate frequency region of the modulus curves (Figs.1(c) and (d)) of the dispersion-strengthened high-strength steel with longer wetting time (cycle II) were closer to ?1.

    When the drying time was longer (cycle I), it could be seen in the phase angle plot (Fig.1(e)) that with the extension of the corrosion time, the phase angle peak gradually shifted to the low frequency region. This showed that although the corrosion products of the dispersion-streng- thened high-strength steel have increased, its compactness did not increase; However, when the wetting time was longer (cycle II), in the first 10d of corrosion, the phase angle peaks (Fig.1(f)) moved to the low frequency area, and then the phase angle peaks position did not change much. The above showed that in wet-dry cycling environ- ments, an environment with longer wetting time was more conducive to the generation of dense corrosion products.

    Fig.1 EIS plots of dispersion-strengthened high-strength steel under two wet-dry cycling environments. (a, c, e) Nyquist plot, Modulus plot, Phase angle plot under Cycle I; (b, d, f) Nyquist plot, Modulus plot, Phase angle plot under Cycle II.

    In the environment of longer drying time (cycle I), the corrosion products on the surface were less after 5d of corrosion. The EIS plots were fitted by the equivalent circuit diagram shown in Fig.2(a). After 10d of corrosion, Warburg impedance could be seen from the Nyquist diagram (Fig.1(a)), and the rust layer was stratified. Therefore, the equivalent circuit diagram shown in Fig.2 (c) was used for fitting, and the fitting results were listed in Table 3. In the environment of longer wetting time (cycle II), the EIS plots of the first 10d of corrosion were fitted by the equivalent circuit diagram shown in Fig.2(a). With the increase of corrosion products on the surface, the rust layer began to be divided into inner and outer layers. The equivalent circuit diagram shown in Fig.2(b) was used for fitting when the corrosion lasts for 15 to 25d. Warburg impedance appeared after 30d of corrosion (Fig.1(b)), so the equivalent circuit diagram shown in Fig.2(c) was used for fitting. Fitting results were listed in Table 4.

    Fig.2 Equivalent circuits used to fit the EIS measurement.

    Table 3 The electrochemical parameters fitted from the EIS data of dispersion-strengthened high-strength steel at different corrosion time under cycle I

    Table 4 The electrochemical parameters fitted from the EIS data of dispersion-strengthened high-strength steel at different corrosion time under cycle II

    The impedance of a CPE is a function of the frequency and it is defined as:

    whereCPEwas the magnitude of CPE, Ω?1scm?2;was the square root of ?1;was the angular frequency, rads?1; and the exponent(?1≤≤ 1) denoted the distribution of time constant.

    It could be seen from the fitting results that thectof the dispersion-strengthened high-strength steel were larger under the environment of cycle II, which indicated that the corrosion rate of the high strength steel was slow when the wetting time was longer. The change of surface rust resistance of dispersion-strengthened high-strength steel in two environments were shown in Fig.3. Fig.3(a) showed that the resistance of inner and outer rust layer decreased with the increase of corrosion time under longer drying time environment (cycle I). It showed that the protection of rust layer decreased with the increase of corrosion time. However, the resistance of inner and outer rust layers showed different tendency in the environment of longer wetting time (cycle II) (Fig.3(b)). With the increase of corrosion time, the resistance of outer rust layer decreased and the resistance of inner rust layer increased. The results showed that a longer wetting time promoted the formation of dense inner rust layer, which played a protective role for the dispersion-strengthened high- strength steel in wet-dry alternate environment.

    Fig.3 Change of inner and outer rust layer resistance. (a), cycle I; (b), cycle II.

    3.2 The Effect of Wet-Dry Cycling on Pitting Corrosion

    In order to observe the pitting corrosion on the surface of dispersion-strengthened high-strength steel, the corroded steel was derusted and observed by LCSM. Fig.4 showed the 3D morphologies of the dispersion-streng- thened high-strength steel after 15d and 30d of corrosion in two environments. The blue areas were the corrosion pits and the red areas were the platforms. Under the condition of a longer drying time (cycle I), there were many large and deep corrosion pits on the surface of dispersion-strengthened high-strength steel. As the corrosion time increased, the depth of the corrosion pits increased. The surfaces of high-strength steel were relatively smooth under the condition of a longer wetting time (cycle II), and the size and depth of corrosion pits were significantly smaller. The corrosion pits information of dispersion- strengthened high-strength steel under different environments were summarized in Table 5.

    Fig.4 3D images of dispersion-strengthened high-strength steel under two wet-dry cycling environments. (a), 15d under cycle I; (b), 30d under cycle I; (c), 15d under cycle II; (d), 30d under cycle II.

    Through Table 5 we could intuitively understand the corrosion pits information of the dispersion-strengthened high-strength steel under the two wet-dry cycling environments. As the corrosion time increased, the pitting of the dispersion-strengthened high-strength steel under the two environments had a development trend, and the depth and the size were expanding. However, after corrosion for the same time, the maximum pit depth and the equivalent diameter of the pits were significantly larger in the environment with a longer drying time (cycle I). The maximum pit depth of steel in the environment of longer drying time (cycle I) was about 10μm larger than that in the environment of longer wetting time (cycle II). The equivalent diameter of the pits in the longer drying time environment (cycle I) was 2–3 times of that in the other environment (cycle II). When the drying time was longer (cycle I), the maximum depth of the pits and the diameter of the corrosion pits were larger than when the wetting time was longer (cycle II), but the density of pitting corrosion was lower. It might be that multiple corrosion pits gradually developed and connected after drying for a longer time. As a result, the number of pits decreased.

    Table 5 Information on pits of dispersion-strengthened high-strength steel

    3.3 The Effect of Wet-Dry Cycling on the Rust Layer

    3.3.1 Analysis of rust layer morphologies

    The process of wet-dry cycling was essentially a process of changing the thickness of the thin liquid film on the metal surface. The reduction reaction of dissolved oxygen in the thin liquid film at different stages also leaded to a step change in the corrosion potential. The rust layer also had a great influence on the corrosion process. As the corrosion progressed the rust layer became thicker, and the seawater in the rust layer took longer to evaporate. Therefore, the outer rust layer directly affected the wetting time of the metal surface.

    Fig.5 Corrosion product morphologies of dispersion-strengthened high-strength steel under two wet-dry cycling environments. (a–d) 15d inner layer, 15d outer layer, 30d inner layer, 30d outer layer under cycle I; (e–h) 15d inner layer, 15d outer layer, 30d inner layer, 30d outer layer under cycle II.

    Fig.5 was the morphologies of the inner and outer layers of the corrosion products of the dispersion-streng- thened high-strength steel corroded for 15 and 30d under two wet-dry cycling environments. When the drying time was longer (cycle I), after 15d of corrosion, the inner and outer rust layers were loose. The shape of the rust layer was granular and had many gaps and holes. The existence of these gaps and holes provided a powerful transmission channel for dissolved oxygen and corrosive ions in seawater. The looseness of the rust layer increased its water retention, so that the surface of the dispersion-streng- thened high-strength steel remained wet for a long time. Therefore, when the drying time was longer (cycle I), the loose rust layer promoted corrosion after 15d of corrosion. When the wetting time was longer (cycle II), the inner rust layer after 15d was lumpy and granular, and the outer rust layer was granular and piled up in clumps. The rust layer was densely packed and had few holes, which hindered the progress of corrosion to a certain extent. After 30d of corrosion, the density of the inner rust layer had increased under the environment of a longer drying time (cycle I), but it could be seen that the outer rust layer was still relatively loose and could store more seawater. However, the inner and outer rust layers were denser under the environment of longer wetting time (cycle II) which could protect the steel to a certain extent. Therefore, from the perspective of the protection of the rust layer, when the wetting time was longer (cycle II), the rust layer was denser, with fewer gaps and holes and better protection. Therefore, it could prevent the corrosive ions and dissolved oxygen in the seawater from penetrating the rust layer to the steel surface, preventing the further occurrence of pitting corrosion of the dispersion-streng- thened high-strength steel. That was consistent with the results of EIS.

    3.3.2 Analysis of rust layer compositions

    Stratmann. (1990) pointed out that the protective properties of the rust layer depended on its chemical composition, adhesion, compactness and moisture absorption capacity. In the wet-dry cycling environment, rust layer acted as a strong oxidant, which could promote electrochemical reactions under wet or humid stages (Thee., 2014). Raman spectroscopy was used to analyze the compositions of the rust of the dispersion-streng- thened high-strengthened steel in two wet-dry cycling en- vironments for different times. The results were shown in Figs.6 and 7. It could be seen that the corrosion products of dispersion-strengthened high-strength steel in wet-dry cycling environment were mainly Fe3O4and γ-FeOOH. The corrosion product compositions under different conditions were summarized in Table 6. After 15d of corrosion, a small amount of β-FeOOH appeared in the corrosion products in both environments. When the drying time was longer (cycle I), β-FeOOH was in the inner rust layer. However, when the wetting time was longer (cycle II), β-FeOOH only existed in the outer rust layer. β-FeOOH was formed in the presence of chloride ions and under low pH environment (Nomura., 1988). Combined with the corrosion product morphology diagrams in Fig.5, when the drying time was longer (cycle I), the outer rust layer was very loose. Cl?could penetrate the loose outer rust layer to the inside of the rust layer, and reacted with the inner rust layer to form β-FeOOH. The crystal structure of β-FeOOH had holes like tunnels, and Cl?could be filled in the holes to form basic hydrox- ides with chlorine (Deliyanni., 2001). Nishimura. (1995) believed that β-FeOOH was loose and had low adhesion. β-FeOOH could turn into a green layer in the dry period in a wet-dry cycling environment containing Cl?. Therefore, β-FeOOH would destroy the protective of the rust layer and accelerate the corrosion rate of steel.

    Table 6 Summary of corrosion products compositions under two wet-dry cycling environments

    Fig.6 Raman diagrams of rust layercompositions of dispersion-strengthened high-strength steel under cycle I environment. (a), 15d; (b), 30d.

    Fig.7 Raman diagrams of rust layer compositions of dispersion-strengthened high-strength steel under cycle II environment. (a), 15d; (b), 30d.

    The anodic reaction on the surface of dispersion- strengthened high-strength steel at the initial stage of corrosion was the dissolution of iron and the depolarization reaction of oxygen at the cathode, as shown in formulas 2 and 3.

    With the progress of the corrosion electrochemical reaction, the rust layer on the surface of the steel gradually grew and increased, and the rust layer also began to participate in the reaction. The corrosion process of the steel surface under the wet-dry cycling marine environment could be divided into the following three processes (Yadav., 2004; Morcillo., 2014):

    1) Surface wetting process

    During the transition from the dry state to the wet state, the anode reaction was the dissolution of iron, and the cathodic reaction was the reduction of γ-FeOOH in the rust layer (Evans and Taylor, 1972).

    2) Complete surface wetting stage

    When in a wet state, after the γ-FeOOH that could be reduced was consumed, the reduction of dissolved oxygen became the main reaction of the cathode. In this process, the rust layer was filled with electrolyte, which was not conducive to the diffusion of O2, so the corrosion rate was slow. The dissolution rate of the metal depended on the limiting diffusion current density of the O2reduction reaction in the pore electrolyte of the rust layer. The cathode reaction was as follows:

    3) Surface drying process

    In the process of transition from the wet state to the dry state, the thin liquid film on the surface of the rust layer was getting thinner and thinner. A large amount of O2was supplied through the thin liquid film, and the diffusion of O2was accelerated, and the corrosion rate was accelerated. O2reduction reaction occurred during the cathode process, and γ-Fe·OH·OH would be oxidized to γ-FeOOH. The reaction formula was as follows:

    In the wet-dry cycling environment, the components of the rust layer were mutually transformed. The reduction ability of the components in the rust layer was β-FeOOH>γ-FeOOH>α-FeOOH (Lair., 2006). The electrochemical reactions involved in the conversion of the rust layer were mainly γ-FeOOH and Fe3O4. When the drying time was longer (cycle I), the γ-FeOOH in the rust layer was more than another environment and Fe3O4showed the opposite trend. The reason was that in the wet stage of the wet-dry cycling environment, the process of converting γ-FeOOH to Fe3O4mainly occurred, and vice versa in the dry stage (Matsushima, 2004).

    After 30d of corrosion, the types of corrosion products generated in the two environments were the same. When the wetting time was longer (cycle II), the α-FeOOH in the rust layer was only detected in the inner rust layer. α-FeOOH had a stable structure and was difficult to undergo electrochemical reactions, and to a certain extent, so it could protect the dispersion-strengthened high- strength steel from corrosion.

    3.4 The Effect of Wet-Dry Cycling on the Secondary Distribution of Alloying Elements

    The alloying elements added to the high-strength steel played an important role in its corrosion resistance. The alloying elements had different solubility in the steel and the rust layer (Zhou., 2013). As the corrosion progressed, the alloying elements would undergo secondary distribution in the corrosion products. EMPA was used to observe the distributions of alloying elements in the rust layer, as shown in Fig.8. The left side of each figure was a cross-sectional view of the rust layer, and the right side was the element distribution in the red frame of the rust layer section. It could be seen from the cross section of the rust layer that the longer the drying time (cycle I), the thicker the rust layer. It could also indicate that the corrosion of dispersion-strengthened high-strength steel was more serious when the drying time was longer (cycle I). After 15d of corrosion with longer drying time, Cr, Ni, Mo and Cl elements were concentrated in the boundary area between the inner and outer rust layers. After 30d of corrosion with longer drying time, Cr, Ni and Mo elements ‘diffused’ from the inner rust to the outer rust, and the distribution areas increased. On the other hand, in the environment with longer wetting time (cycle II), enrichment zones of Cr, Mg and Mo appeared at the junction of inner and outer rust layer at 15d. Ni were distributed throughout the rust layer, but mainly concentrated in the inner rust layer. The enrichment of alloy elements at the junction of inner and outer rust layer could hinder the diffusion of the external corrosive medium to the steel, hinder the further growth of the rust layer grains and make the rust layer grew dense. At 30d of corrosion with longer wetting time, the enrichment zones disappeared. Cr and Ni elements were mainly concentrated in the internal rust, and Mo elements were distributed throughout the rust layer. At this time, the Cl element detected in the rust layer was very little. Therefore, in a longer wetting time environment (cycle II), during the secondary distribution of alloying elements, the alloying elements were easily concentrated in the internal rust layer.

    It could be seen from the Fig.6 that the distribution of Ni element and Cl element were opposite to each other. Nishimura. (2003)believed that the alloying element Ni easily entered the rust layer during the corrosion process and formed a spinel oxide NiFe2O4with the same structure as Fe3O4. Compared with Fe3O4, NiFe2O4had higher thermodynamic and electrochemical stability, which was beneficial to reduce the corrosion rate. In addition, studies had shown that NiFe2O4had cation selective permeability, which could prevent Cl?in the marine passing through the rust layer to the surface of the steel. This could prevent Cl?from inducing pitting corrosion of the dispersion-strengthened high-strength steel. It showed that under the environment with a longer wetting time (cycle II), the alloying elements concentrated inside the rust layer during the secondary distribution, and increased the protective of the rust layer. Cr element was more likely to produce a certain degree of element segregation in the rust layer, which could repair defects such as pores and cracks in the rust layer and enhance the compactness of the rust layer (Chai., 2016; Jung., 2018). The Cr element was mainly distributed in the inner rust layer and the interface between the inner and outer rust layers. The enrichment of the Cr element in the inner rust layer would reduce the degree of crystallization of corrosion products, refine the rust layer and promote the formation of α-FeOOH. In this process, the secondary distribution of Cr promoted the increase of α-FeOOH and Fe3O4in the inner rust layer. So the inner rust layer contained less γ-FeOOH and more Fe3O4.

    Fig.8 EMPA diagrams of cross-section elementdistributions of rust layer of dispersion-strengthened high-strength steel under two wet-dry cycling environments. (a), 15d under cycle I; (b), 30d under cycle I; (c), 15d under cycle II; (d), 30d under cycle II.

    4 Conclusions

    The control steps of the electrochemical reaction were different in the two marine wet-dry cycling environments. After 10d of corrosion with a longer drying time (cycle I), the electrochemical process was jointly controlled by charge transfer process and diffusion process. The electrochemical process was controlled by charge transfer and diffusion after 30d of corrosion when the wetting time was longer (cycle II). Before that, the electrochemical process was only controlled by charge transfer process. The pitting corrosion of dispersion-strengthened high- strength steel was more serious when the drying time was longer (cycle I). However, when the wetting time was longer (cycle II), the high-strength steel corroded slightly, and the size and depth of the corrosion pits on the surface were small. This was because in an environment with a longer wetting time (cycle II), the dispersion-strengthened high-strength steel could be promoted to generate denser corrosion products. It could promote the conversion of γ-FeOOH to Fe3O4in the rust layer and the formation of α-FeOOH in the inner rust layer. In addition, it also promoted the concentration of Cr, Ni, Mo alloying elements in the inner rust layer. Due to the above reasons, the dissolved oxygen and Cl?were prevented from penetrating the rust layer into the surface of the dispersion-streng- thened high-strength steel, which reduced the further occurrence of pitting corrosion.

    Acknowledgement

    The study is supported by the National Natural Science Foundation of China (No. U1706221).

    Chai, F., Jiang, S., and Yang, C. F., 2016. Effect of Cr on characteristic of rust layer formed on low alloy steel in flow-accelerated corrosion environment., 23 (6): 602-607.

    Chen, Y. Y., Tzeng, H. J., Wei, L. I., Oung, J. C., and Shin, H. C., 2005. Corrosion resistance and mechanical properties of low-alloy steels under atmospheric conditions., 47 (4): 1001-1021.

    Deliyanni, E. A., Bakoyannakis, D. N., Zouboulis, A. I., Matis, K. A., and Nalbandian, L., 2001. Akaganeite-type β-FeOOH nanocrystals: Preparation and characterization., 42 (1): 49.

    Díaz, I., Cano, H., Lopesino, P., de la Fuente, D., Chico, B., Jiménez, J. A.,., 2018. Five-year atmospheric corrosion of Cu, Cr and Ni weathering steels in a wide range of environments., 141: 146-157.

    Evans, U., and Taylor, C., 1972. Mechanism of atmospheric rusting., 12 (3): 227-246.

    Jung, K. M., Ahn, S. H., Kim, Y. J., Oh, S. K., Ryu, W. H., and Kwon, H. S., 2018. Alloy design employing high Cr concentrations for Mo-free stainless steels with enhanced corrosion resistance., 140: 61-72.

    Lair, V., Antony, H., Legrand, L., and Chausse, A., 2006. Electrochemical reduction of ferric corrosion products and evaluation of galvanic coupling with iron., 48 (8): 2050-2063.

    Matsushima, R., translated by Jing, Y. K., 2004.. Metallurgical Industry Press, Beijing,230pp.

    Morcillo, M., Díaz, I., Chico, B., Cano, H., and Fuente, D., 2014. Weathering steels: From empirical development to scientific design, a review., 83 (7): 6-31.

    Nishimura, T., and Kodama, T., 2003. Clarification of chemical state for alloying elements in iron rust using a binary-phase potential-pH diagram and physical analyses., 45 (5): 1073-1084.

    Nishimura, T., Noda, K., and Kodama, T., 2001. Corrosion behavior of tungsten-bearing steel in a wet/dry environment containing chloride ions., 57 (9): 753-758.

    Nishimura, T., Tanaka, K., and Shimizu, Y., 1995. Effect of NaCl on rusting of steel in wet and dry corrosion cycle., 81 (11): 1079-1084.

    Nomura, K., Tasaka, M., and Ujihira, Y., 1988. Conversion electron Mossbauer spectrometric study of corrosion products of iron immersed in sodium chloride solution., 44 (3): 131-135.

    Park, I. J., Lee, S. M., Kang, M. W., Lee, S. J., and Lee, Y. K., 2015. Pitting corrosion behavior in advanced high strength steels., 619: 205-210.

    Porcayo, C., Rivera, M. J., Peza-Ledesma, E. M., Casales-Diaz, C., and Martinez-Gomez, M. L., 2017. Sustainable development of palm oil: Synthesis and electrochemical performance of corrosion inhibitor., 8: 133.

    Soltis, J., 2015. Passivity breakdown, pit initiation and propagation of pits in metallic materials – Review., 90: 5-22.

    Stratmann, M., Bohnenkamp, K., and Engell, H. J., 1989. An electrochemical study of phase-transitions in rust layers., 23 (9): 969-985.

    Stratmann, M., and Streckel, H., 1990. On the atmospheric corrosion of metals which are covered with thin electrolyte layers-I. Verification of the experimental technique., 30 (6-7): 681-696.

    Thee, C., Hao, L., Dong, J. H., Mu, X., Wei, X., Li, X. F., and Ke, W., 2014. Atmospheric corrosion monitoring of a weathering steel under an electrolyte film in cyclic wet-dry condition., 78: 130-137.

    Wang, L. W., Xin, J. C., Cheng, L. J., Zhao, K., Sun, B. Z., Li, J. R.,., 2019. Influence of inclusions on initiation of pitting corrosion and stress corrosion cracking of X70 steel in near-neutral pH environment., 147: 108- 127.

    Wang, Y. F., Cheng, G. X., Wu, W., and Qiao, Q., 2015. Effect of pH and chloride on the micro-mechanism of pitting corrosion for high strength pipeline steel in aerated NaCl solutions., 349: 746-756.

    Yadav, A. P., Nishikata, A., and Tsuru, T., 2004. Electrochemical impedance study on galvanized steel corrosion under cyclic wet-dry conditions-influence of time of wetness., 46 (1): 169-181.

    Yu, J. X., Wang, H. K., Yu, Y., Luo, Z., Liu, W. D., and Wang, C. M., 2018. Corrosion behavior of X65 pipeline steel: Comparison of wet-dry cycle and full immersion., 133: 276-287.

    Zhang, B., and Ma, X. L., 2019.A review–Pitting corrosion initiation investigated by TEM., 35: 1455-1465.

    Zhou, Y. L., Chen, J., Xu, Y., and Liu, Z. Y., 2013. Effects of Cr, Ni and Cu on the corrosion behavior of low carbon microalloying steel in a Cl?containing environment., 29 (2): 168-174.

    November 16, 2020;

    April 17, 2021;

    June 8, 2021

    ? Ocean University of China, Science Press and Springer-Verlag GmbH Germany 2021

    . Tel: 0086-532-66781637

    E-mail: ssdm99@ouc.edu.cn

    (Edited by Ji Dechun)

    成人午夜精彩视频在线观看| 日本欧美国产在线视频| 亚洲少妇的诱惑av| 亚洲成色77777| 男女啪啪激烈高潮av片| 国产成人精品婷婷| 国产片特级美女逼逼视频| 久久精品国产鲁丝片午夜精品| 在线精品无人区一区二区三| 只有这里有精品99| 国产人伦9x9x在线观看 | 岛国毛片在线播放| 五月伊人婷婷丁香| 亚洲,一卡二卡三卡| 三级国产精品片| 久久国产亚洲av麻豆专区| 久久久久国产精品人妻一区二区| 午夜福利一区二区在线看| 永久网站在线| 少妇的丰满在线观看| 亚洲婷婷狠狠爱综合网| 亚洲少妇的诱惑av| 亚洲欧美精品自产自拍| 成人国语在线视频| 在线 av 中文字幕| 日韩一区二区视频免费看| 免费观看在线日韩| 2018国产大陆天天弄谢| 亚洲国产最新在线播放| 久久久国产欧美日韩av| 香蕉丝袜av| 精品久久久久久电影网| 日韩欧美精品免费久久| 伊人久久大香线蕉亚洲五| 久久精品国产亚洲av涩爱| 免费高清在线观看视频在线观看| 人人澡人人妻人| 国产精品国产三级国产专区5o| 日韩一区二区视频免费看| 边亲边吃奶的免费视频| 国产亚洲欧美精品永久| 最近2019中文字幕mv第一页| 美女视频免费永久观看网站| 精品人妻在线不人妻| 成人免费观看视频高清| 亚洲精品视频女| 免费av中文字幕在线| 国产 精品1| 青春草视频在线免费观看| 寂寞人妻少妇视频99o| 免费不卡的大黄色大毛片视频在线观看| 久久午夜福利片| 男人舔女人的私密视频| 成人免费观看视频高清| 中文字幕色久视频| 日韩 亚洲 欧美在线| 日韩视频在线欧美| 18在线观看网站| 国产人伦9x9x在线观看 | 日韩精品有码人妻一区| 美女福利国产在线| 国产亚洲av片在线观看秒播厂| 国产男女超爽视频在线观看| 国产一区亚洲一区在线观看| 亚洲综合精品二区| 欧美在线黄色| 欧美亚洲 丝袜 人妻 在线| 国产片内射在线| 狂野欧美激情性bbbbbb| 午夜福利,免费看| 免费人妻精品一区二区三区视频| 久久青草综合色| 丝袜在线中文字幕| 捣出白浆h1v1| 日本vs欧美在线观看视频| 国产免费一区二区三区四区乱码| 国产日韩欧美在线精品| a级毛片在线看网站| 夫妻午夜视频| 欧美成人精品欧美一级黄| 99国产精品免费福利视频| 欧美精品一区二区免费开放| 毛片一级片免费看久久久久| 老熟女久久久| 精品福利永久在线观看| 久久午夜综合久久蜜桃| 热re99久久精品国产66热6| 亚洲在久久综合| 国产精品一国产av| xxxhd国产人妻xxx| 丁香六月天网| 一级,二级,三级黄色视频| 97在线视频观看| 99热全是精品| 五月开心婷婷网| 日韩一卡2卡3卡4卡2021年| 亚洲国产最新在线播放| 美女中出高潮动态图| 精品人妻偷拍中文字幕| 91在线精品国自产拍蜜月| 精品99又大又爽又粗少妇毛片| 国产免费现黄频在线看| 久久久国产一区二区| 欧美日韩av久久| 亚洲欧美成人精品一区二区| 精品国产乱码久久久久久小说| 精品卡一卡二卡四卡免费| 97在线人人人人妻| 日韩人妻精品一区2区三区| 91久久精品国产一区二区三区| 久久精品久久久久久久性| 久久久久精品人妻al黑| 色吧在线观看| 人妻系列 视频| 伦精品一区二区三区| 少妇被粗大猛烈的视频| 亚洲精品日本国产第一区| 久久这里有精品视频免费| 午夜日本视频在线| 嫩草影院入口| 久热这里只有精品99| 18在线观看网站| 日本爱情动作片www.在线观看| 国产深夜福利视频在线观看| 天堂中文最新版在线下载| 爱豆传媒免费全集在线观看| 最近的中文字幕免费完整| 尾随美女入室| 日韩大片免费观看网站| 九色亚洲精品在线播放| 黄色一级大片看看| 国产成人精品婷婷| 亚洲国产成人一精品久久久| 午夜福利在线观看免费完整高清在| 男女边吃奶边做爰视频| 妹子高潮喷水视频| 久久久久久久久久人人人人人人| 夫妻午夜视频| 韩国精品一区二区三区| 日韩人妻精品一区2区三区| 人人澡人人妻人| 久久精品国产亚洲av天美| 欧美日韩一区二区视频在线观看视频在线| 久久ye,这里只有精品| 99热全是精品| 美女脱内裤让男人舔精品视频| 亚洲欧美精品自产自拍| 97在线视频观看| 美女视频免费永久观看网站| 久久99一区二区三区| 欧美少妇被猛烈插入视频| 婷婷成人精品国产| 日本-黄色视频高清免费观看| av免费观看日本| 美国免费a级毛片| 久久精品熟女亚洲av麻豆精品| 亚洲精品自拍成人| 美女福利国产在线| 午夜免费男女啪啪视频观看| 看非洲黑人一级黄片| 亚洲综合精品二区| 99国产精品免费福利视频| 色婷婷av一区二区三区视频| 国产精品国产三级国产专区5o| 国产精品.久久久| av又黄又爽大尺度在线免费看| 国产精品免费视频内射| 国产免费现黄频在线看| av天堂久久9| 中文字幕制服av| 日本免费在线观看一区| 天堂8中文在线网| 久久精品国产鲁丝片午夜精品| 交换朋友夫妻互换小说| 精品少妇内射三级| 熟女av电影| 国产麻豆69| 中文乱码字字幕精品一区二区三区| kizo精华| 日韩不卡一区二区三区视频在线| 韩国av在线不卡| videosex国产| 中国国产av一级| 国产在线一区二区三区精| 成人毛片a级毛片在线播放| 欧美日韩视频高清一区二区三区二| 日日啪夜夜爽| 亚洲色图 男人天堂 中文字幕| 王馨瑶露胸无遮挡在线观看| 久久毛片免费看一区二区三区| 最新中文字幕久久久久| 97精品久久久久久久久久精品| 黄色配什么色好看| 又粗又硬又长又爽又黄的视频| 国产无遮挡羞羞视频在线观看| 精品国产一区二区三区久久久樱花| 亚洲内射少妇av| 久久久久久人人人人人| 男女啪啪激烈高潮av片| 99久久综合免费| 久久这里有精品视频免费| av福利片在线| 精品少妇一区二区三区视频日本电影 | 国产免费又黄又爽又色| 中文字幕人妻熟女乱码| 亚洲五月色婷婷综合| 五月开心婷婷网| 有码 亚洲区| 男人舔女人的私密视频| 青草久久国产| 久久久久网色| 国产av码专区亚洲av| 久久ye,这里只有精品| 高清在线视频一区二区三区| 69精品国产乱码久久久| 少妇 在线观看| videosex国产| 精品少妇久久久久久888优播| 一级爰片在线观看| 日韩精品有码人妻一区| 啦啦啦啦在线视频资源| 日韩一本色道免费dvd| 高清不卡的av网站| 日韩在线高清观看一区二区三区| 女人精品久久久久毛片| 国产爽快片一区二区三区| 边亲边吃奶的免费视频| 国产成人a∨麻豆精品| 午夜福利乱码中文字幕| 亚洲成国产人片在线观看| 亚洲三区欧美一区| 成人毛片60女人毛片免费| 最近中文字幕高清免费大全6| 美女午夜性视频免费| 日韩中字成人| 热re99久久精品国产66热6| 亚洲欧美一区二区三区黑人 | 你懂的网址亚洲精品在线观看| 综合色丁香网| 午夜福利乱码中文字幕| 成年女人毛片免费观看观看9 | av在线播放精品| 精品一品国产午夜福利视频| 一级毛片 在线播放| 亚洲精品在线美女| 亚洲av国产av综合av卡| 女性被躁到高潮视频| 免费大片黄手机在线观看| 国产激情久久老熟女| 伊人久久大香线蕉亚洲五| freevideosex欧美| a 毛片基地| 大陆偷拍与自拍| 精品第一国产精品| 精品一品国产午夜福利视频| 大码成人一级视频| 美女视频免费永久观看网站| 伊人亚洲综合成人网| 少妇猛男粗大的猛烈进出视频| 久久久精品免费免费高清| 亚洲国产av影院在线观看| 一边摸一边做爽爽视频免费| 交换朋友夫妻互换小说| 国产精品嫩草影院av在线观看| 亚洲国产日韩一区二区| 亚洲情色 制服丝袜| 男人添女人高潮全过程视频| 成年女人毛片免费观看观看9 | videossex国产| 亚洲成av片中文字幕在线观看 | av在线app专区| av免费观看日本| 免费黄色在线免费观看| 美女大奶头黄色视频| 丝袜美足系列| 亚洲在久久综合| 丰满乱子伦码专区| 亚洲欧美色中文字幕在线| 亚洲欧美成人综合另类久久久| 久久人人爽人人片av| 免费观看在线日韩| 最近手机中文字幕大全| 性高湖久久久久久久久免费观看| xxxhd国产人妻xxx| 99re6热这里在线精品视频| 午夜激情久久久久久久| www.自偷自拍.com| 日韩伦理黄色片| 日韩中文字幕欧美一区二区 | 99精国产麻豆久久婷婷| 卡戴珊不雅视频在线播放| 高清视频免费观看一区二区| 成人漫画全彩无遮挡| 亚洲国产看品久久| 777米奇影视久久| 女的被弄到高潮叫床怎么办| 视频在线观看一区二区三区| 少妇 在线观看| 最近最新中文字幕大全免费视频 | 在线观看美女被高潮喷水网站| 久久这里有精品视频免费| 18禁裸乳无遮挡动漫免费视频| 久久久久久久大尺度免费视频| 亚洲精品自拍成人| 免费黄色在线免费观看| 亚洲av中文av极速乱| 女性被躁到高潮视频| 国产av码专区亚洲av| 91精品伊人久久大香线蕉| 日本黄色日本黄色录像| 最近中文字幕高清免费大全6| 蜜桃在线观看..| av又黄又爽大尺度在线免费看| 国产乱人偷精品视频| 日本色播在线视频| 亚洲av综合色区一区| 午夜福利网站1000一区二区三区| av不卡在线播放| 最近中文字幕2019免费版| 国产免费视频播放在线视频| 久久久久久久久久久免费av| 嫩草影院入口| 亚洲成人av在线免费| xxxhd国产人妻xxx| 看免费成人av毛片| 国产成人免费无遮挡视频| 精品少妇黑人巨大在线播放| 久久人人爽av亚洲精品天堂| 国产伦理片在线播放av一区| 久久热在线av| 亚洲,欧美精品.| 丰满乱子伦码专区| 久久婷婷青草| 欧美少妇被猛烈插入视频| 精品视频人人做人人爽| 国产男人的电影天堂91| 国产精品香港三级国产av潘金莲 | 日韩不卡一区二区三区视频在线| 欧美成人午夜免费资源| 精品一区二区免费观看| 国产乱人偷精品视频| 国产精品秋霞免费鲁丝片| 香蕉精品网在线| 亚洲熟女精品中文字幕| 亚洲av综合色区一区| 国产黄频视频在线观看| 黄网站色视频无遮挡免费观看| 日韩人妻精品一区2区三区| 男人爽女人下面视频在线观看| 香蕉丝袜av| 精品久久久精品久久久| 老司机影院毛片| 大片免费播放器 马上看| 国产欧美亚洲国产| 精品少妇内射三级| 国产精品av久久久久免费| 在线观看免费高清a一片| 精品人妻熟女毛片av久久网站| 色视频在线一区二区三区| 国产毛片在线视频| 久久精品久久精品一区二区三区| 黄色配什么色好看| 亚洲成人手机| 久久精品人人爽人人爽视色| av国产久精品久网站免费入址| 亚洲经典国产精华液单| 国产免费一区二区三区四区乱码| 香蕉丝袜av| 国语对白做爰xxxⅹ性视频网站| 90打野战视频偷拍视频| 毛片一级片免费看久久久久| 99国产综合亚洲精品| 好男人视频免费观看在线| 老司机影院毛片| 欧美日韩国产mv在线观看视频| 成人亚洲欧美一区二区av| 亚洲成人手机| 你懂的网址亚洲精品在线观看| 高清欧美精品videossex| 免费观看在线日韩| 亚洲国产精品成人久久小说| 麻豆av在线久日| 秋霞在线观看毛片| 亚洲色图 男人天堂 中文字幕| 老汉色∧v一级毛片| 国产精品成人在线| 国产一级毛片在线| 99香蕉大伊视频| 三上悠亚av全集在线观看| 看非洲黑人一级黄片| 久久久久久人妻| 国产精品秋霞免费鲁丝片| 高清在线视频一区二区三区| 精品久久蜜臀av无| 精品一品国产午夜福利视频| 在线观看国产h片| 欧美老熟妇乱子伦牲交| 久久99热这里只频精品6学生| 亚洲国产日韩一区二区| 精品国产国语对白av| 国产精品一区二区在线观看99| 精品少妇内射三级| 亚洲第一区二区三区不卡| 色婷婷久久久亚洲欧美| 久久免费观看电影| 婷婷色av中文字幕| 久久久久精品久久久久真实原创| 乱人伦中国视频| 日韩大片免费观看网站| 秋霞伦理黄片| 天堂8中文在线网| 欧美激情极品国产一区二区三区| 午夜老司机福利剧场| 天堂中文最新版在线下载| 曰老女人黄片| 久久精品亚洲av国产电影网| 丝袜在线中文字幕| 亚洲综合色惰| 久久婷婷青草| 9色porny在线观看| 大香蕉久久网| 精品久久久精品久久久| 中文天堂在线官网| 欧美成人午夜精品| 精品国产乱码久久久久久小说| 99久久人妻综合| 成年女人毛片免费观看观看9 | 侵犯人妻中文字幕一二三四区| 日韩av在线免费看完整版不卡| 亚洲五月色婷婷综合| 国产精品一国产av| 久久精品国产鲁丝片午夜精品| 日韩三级伦理在线观看| 久久精品aⅴ一区二区三区四区 | 国产淫语在线视频| 成人影院久久| 不卡视频在线观看欧美| 人妻人人澡人人爽人人| 男的添女的下面高潮视频| 侵犯人妻中文字幕一二三四区| 如日韩欧美国产精品一区二区三区| 如何舔出高潮| 国产成人91sexporn| 巨乳人妻的诱惑在线观看| 多毛熟女@视频| 欧美+日韩+精品| 啦啦啦视频在线资源免费观看| 免费高清在线观看日韩| 国产精品嫩草影院av在线观看| 亚洲精品自拍成人| 纯流量卡能插随身wifi吗| 国产一区二区在线观看av| 波多野结衣av一区二区av| 国产亚洲欧美精品永久| 深夜精品福利| 国产精品久久久久久av不卡| 国产成人精品无人区| 一级a爱视频在线免费观看| 日韩av不卡免费在线播放| 久久精品久久久久久久性| 日韩不卡一区二区三区视频在线| 精品国产一区二区三区四区第35| 久久热在线av| 免费高清在线观看日韩| 国产 精品1| 制服诱惑二区| 久久久国产欧美日韩av| 国产人伦9x9x在线观看 | www日本在线高清视频| 男女边摸边吃奶| 欧美 日韩 精品 国产| 女人精品久久久久毛片| 国产午夜精品一二区理论片| 亚洲色图综合在线观看| 爱豆传媒免费全集在线观看| av线在线观看网站| 久久久精品国产亚洲av高清涩受| 晚上一个人看的免费电影| 亚洲美女黄色视频免费看| 免费黄色在线免费观看| 亚洲一区二区三区欧美精品| 中文字幕制服av| 爱豆传媒免费全集在线观看| 黄片小视频在线播放| 91精品伊人久久大香线蕉| 亚洲av日韩在线播放| 日韩中文字幕欧美一区二区 | 欧美精品一区二区免费开放| 女人高潮潮喷娇喘18禁视频| 国产精品三级大全| 国产在线免费精品| 欧美 亚洲 国产 日韩一| 交换朋友夫妻互换小说| 欧美 日韩 精品 国产| 少妇的丰满在线观看| 亚洲精品一二三| 99久久综合免费| 欧美精品人与动牲交sv欧美| 亚洲成人一二三区av| 国产精品秋霞免费鲁丝片| 在线观看免费视频网站a站| 黄片播放在线免费| 你懂的网址亚洲精品在线观看| 亚洲精品第二区| 亚洲欧洲国产日韩| 成人午夜精彩视频在线观看| 午夜福利视频精品| 国产亚洲欧美精品永久| 91精品三级在线观看| videossex国产| 日韩av不卡免费在线播放| 亚洲精品国产av蜜桃| 欧美日韩亚洲国产一区二区在线观看 | 成人影院久久| 国产高清不卡午夜福利| 亚洲欧美精品综合一区二区三区 | 麻豆乱淫一区二区| 色婷婷av一区二区三区视频| 久久久欧美国产精品| 午夜日韩欧美国产| 天天躁夜夜躁狠狠久久av| 精品99又大又爽又粗少妇毛片| 2018国产大陆天天弄谢| 黄色配什么色好看| 欧美日韩av久久| 日韩伦理黄色片| 日韩精品免费视频一区二区三区| 免费观看无遮挡的男女| 母亲3免费完整高清在线观看 | 久久99精品国语久久久| 国产亚洲精品第一综合不卡| 国产一区二区 视频在线| 香蕉丝袜av| 777久久人妻少妇嫩草av网站| 欧美日韩一级在线毛片| h视频一区二区三区| 久久精品久久精品一区二区三区| 男女下面插进去视频免费观看| 久久久久久免费高清国产稀缺| 国产精品亚洲av一区麻豆 | 波多野结衣一区麻豆| 日本欧美视频一区| 久久97久久精品| 最近最新中文字幕大全免费视频 | 三级国产精品片| 国产97色在线日韩免费| 伦精品一区二区三区| 亚洲四区av| 美女主播在线视频| 午夜免费观看性视频| 中文字幕av电影在线播放| 欧美精品人与动牲交sv欧美| 日韩制服丝袜自拍偷拍| av天堂久久9| 精品国产乱码久久久久久男人| 另类精品久久| 久久久国产一区二区| 精品酒店卫生间| 777久久人妻少妇嫩草av网站| 亚洲欧美成人综合另类久久久| 少妇的逼水好多| 天天躁日日躁夜夜躁夜夜| 久久精品亚洲av国产电影网| 免费少妇av软件| 日本爱情动作片www.在线观看| 亚洲精品aⅴ在线观看| 亚洲国产成人一精品久久久| 欧美国产精品一级二级三级| 午夜福利在线免费观看网站| 国产精品国产三级国产专区5o| 一本色道久久久久久精品综合| 不卡视频在线观看欧美| 人妻少妇偷人精品九色| 亚洲国产av新网站| 少妇的逼水好多| 午夜老司机福利剧场| 日本av免费视频播放| 日韩电影二区| 国产免费一区二区三区四区乱码| 成人手机av| 国产日韩欧美在线精品| 国产免费视频播放在线视频| 18在线观看网站| 91成人精品电影| 久久99热这里只频精品6学生| av网站免费在线观看视频| 亚洲国产精品国产精品| 国产精品女同一区二区软件| 黄频高清免费视频| 国产精品蜜桃在线观看| 国产片内射在线| 免费观看av网站的网址| 三上悠亚av全集在线观看| 成人影院久久| 欧美xxⅹ黑人| 国产精品国产三级国产专区5o| 日韩一卡2卡3卡4卡2021年| 亚洲男人天堂网一区| 免费日韩欧美在线观看| 欧美bdsm另类| 18禁国产床啪视频网站| 热99国产精品久久久久久7| 人人妻人人澡人人看| 热99久久久久精品小说推荐| 国产精品久久久久成人av| 欧美bdsm另类| 熟女av电影| 亚洲国产色片| 亚洲av.av天堂| 亚洲久久久国产精品| 亚洲国产精品成人久久小说| 日日撸夜夜添| 欧美激情极品国产一区二区三区| 麻豆乱淫一区二区| 一级片'在线观看视频|