    Understanding the Role of Cu/ZnO lnteraction in CO2 Hydrogenation to Methanol

    2021-06-02 11:39:42CongmingLiKuoChenXiaoyueWangNanXueHengquanYang
    物理化學(xué)學(xué)報(bào) 2021年5期

    Congming Li , Kuo Chen Xiaoyue Wang Nan Xue , Hengquan Yang ,

    1 Key Laboratory of Coal Science and Technology, Ministry of Education and Shanxi Province, Taiyuan University of Technology,Taiyuan 030024, China.

    2 School of Chemistry and Chemical Engineering, Shanxi University, Taiyuan 030006, China.

    Abstract: Using renewable green hydrogen and carbon dioxide (CO2) to produce methanol is one of the fundamental ways to reduce CO2 emissions in the future, and research and development related to catalysts for efficient and stable methanol synthesis is one of the key factors in determining the entire synthesis process. Metal nanoparticles stabilized on a support are frequently employed to catalyze the methanol synthesis reaction. Metal-support interactions (MSIs) in these supported catalysts can play a significant role in catalysis. Tuning the MSI is an effective strategy to modulate the activity,selectivity, and stability of heterogeneous catalysts. Numerous studies have been conducted on this topic; however, a systematic understanding of the role of various strengths of MSI is lacking. Herein, three Cu/ZnO-SiO2 catalysts with different strengths of MSI, namely, normal precipitation Cu/ZnO-SiO2 (Nor-CZS), co-precipitation Cu/ZnO-SiO2 (Co-CZS), and reverse precipitation Cu/ZnO-SiO2(Re-CZS), were successfully prepared to determine the role of such interactions in the hydrogenation of CO2 to methanol.The results of temperature-programmed reduction (H2-TPR) and X-ray photoelectron spectroscopy (XPS) characterization illustrated that the MSI of the catalysts was considerably affected by the precipitation sequence. Fourier transform infrared reflection spectroscopy (FT-IR) results indicated that the Cu species existed as CuO in all cases and that copper phyllosilicate was absent (except for strong Cu-SiO2 interaction). Transmission electron microscopy (TEM), X-ray diffraction (XRD), and N2O chemical titration results revealed that strong interactions between the Cu and Zn species would promote the dispersion of Cu species, thereby leading to a higher CO2 conversion rate and improved catalytic stability. As expected, the Re-CZS catalyst exhibited the highest activity with 12.4% CO2 conversion, followed by the Co-CZS catalyst(12.1%), and the Nor-CZS catalyst (9.8%). After the same reaction time, the normalized CO2 conversion of the three catalysts decreased in the following order: Re-CZS (75%) > Co-CZS (70%) > Nor-CZS (65%). Notably, the methanol selectivity of the Re-CZS catalyst was found to level off after a prolonged period, in contrast to that of Co-CZS and Nor-CZS. Investigation of the structural evolution of the catalyst with time on stream revealed that the high methanol selectivity of the catalyst was caused by the reconstruction of the catalyst, which was induced by the strong MSI between the Cu and Zn species, and the migration of ZnO onto Cu species, which caused an enlargement of the Cu/ZnO interface. This work offers an alternative strategy for the rational and optimized design of efficient catalysts.

    Key Words: Cu/ZnO-SiO2 catalysts; Metal-support interaction; CO2 hydrogenation; Methanol

    1 lntroduction

    Methanol as an important C1building-block could be converted to various high value-added chemicals. Cu-based catalyst has attracted extensive attention in methanol synthesis because of its excellent redox property, low cost and high recyclability1,2. Among various Cu-based catalysts, Cu/ZnO based catalysts are appealing for the CO2hydrogenation to methanol process due to their unique catalytic properties3,4.

    As a structure-sensitive reaction, catalytic performance of CO2hydrogenation to methanol is significantly affected by catalyst morphology, particle size, crystalline size of support and especially metal-support interaction5. Moreover, depending on the complexity of real systems, dynamic behaviors of structure as well as surface composition observed during reaction process thus affect the nature of active sites and the catalytic performance of Cu-ZnO based catalysts6. Several studies found the directly proportional relationship between methanol synthesis activity and Cu0surface areas (SACu) determined with N2O adsorption7,8. However, taken separately, Cu and ZnO have a low activity for methanol synthesis as well as nonlinearity in correlation of SACuand catalytic activity is often emerged, which indicate the existence of metal-support interaction such as Cu-Zn interaction (CuZn alloy) and Cu-ZnO interaction9. Fujitani et al. observed that Zn is present in the metallic form and proposed that the metallic Cu-Zn alloy is a catalytic active species for the methanol synthesis from CO2and H210. Sebastian et al. supported the formation of a Cu-Zn surface alloy during pretreatment and further found a strong interdependency of methanol synthesis activity and the Zn coverage11.

    On the other hand, Cu-ZnO interaction already acts as a leading proposed model, which exerts a significantly impact on the catalytic performance, such as stability, activity and selectivity via a synergy of Cu and ZnO at the interface,electronic interactions and strong metal-support interactions(SMSI). It is acknowledged that the high-energy sites at the interface are generally accepted as the catalytic sites for methanol synthesis12. Recently, Chen and Rodriguez et al. found that surface Zn transforms into ZnO during CO2hydrogenation to methanol and allows the formation of active Cu-ZnO interface, accompanied with an increase in the catalytic activity for methanol synthesis13. Tsang et al. investigated that morphology effect of ZnO on its interaction with Cu. The results showed that the exposed polar (002) face in platelike ZnO had a much stronger electronic interaction at Cu-ZnO interface,leading to a higher methanol selectivity from CO2and H214. The formation of Cu-ZnO interface drive the transfer of charge from ZnO:Al metal oxide toward Cu metal particles and accumulate at the interface of the Cu-ZnO:Al, which decrease apparent activation energy and increase the reaction order of CO215.Willinger et al. reported that the formation of metastable“graphite-like” ZnO overlayer on Cu nanoparticles induced by strong metal-support interaction (SMSI) during reductive activation. The synergy between Cu and ZnO provide multiple functions in promoting active sites and stabilizing Cu phase mesostructure16. A surface enrichment of Zn in the Cu-ZnOAl2O3catalyst fabricate a unique synergistic Cu-ZnO interaction in boosting CO2hydrogenation and inhibiting RWGS reaction as well as the electronic stabilization of Cu species against reoxidation by CO2and/or H2O, leading to higher activity and methanol selectivity for CO2hydrogenation17. In addition, the dispersion of Cu species could be greatly promoted by the introduction of Zn species, and more synergetic Cu-ZnO sites,therefore, could be exposed to the feed gases leading to a higher reaction activity18. Although the Cu-ZnO interaction has been widely studied, the effect of tuning various strength of metalsupport interaction on catalyst structure and catalytic performance not yet is investigated.

    In the present work, three CuZnO/SiO2catalysts with different strength of metal-support interaction (MSI) were prepared in order to clarify the impact of the interaction between Cu and Zn species on the catalytic performance. The structural evolution of catalyst under the reaction conditions was investigated to establish the relationship between the catalyst structure and catalytic performance. Experimental results suggested that stronger MSI played a critical role in the CO2hydrogenation, and could facilitate the formation of well dispersed metal species thereby affecting the catalytic performance.

    2 Materials and methods

    2.1 Catalyst synthesis

    2.1.1 Normal precipitation method

    10.0 g silica gel (Sigma-Aldrich, 99.9%) was added into a 250 mL beaker containing 200 mL deionized water, which was denoted as suspension A. 6.21 g Cu(NO3)2·3H2O (AR) and 4.12 g Zn(NO3)2·6H2O (AR) were dissolved in deionized water to obtain metal salt solution B ([M2+] = 1 mol·L-1). Initially, the solution B was dropped into the suspension A. After being stirring for 0.5 h, the mixture was heated to 70 °C. Subsequently,a proper amount of Na2CO3(AR) solution (1 mol·L-1) was added into this mixture to adjust the pH to 7. Next, the resultant mixture was further stirred for 1 h and the generated solid was recovered by hot flirtation and washed with deionized water five times. The obtained solid was dried at 60 °C in air overnight and calcined at 350 °C for 4 h, eventually obtaining the catalyst that was denoted as Nor-CZS.

    2.1.2 Co-precipitation method

    10.0 g silica gel (Sigma-Aldrich, 99.9%) was suspended in 200 mL deionized water. After this suspension was heated to 70 °C. A mixture of nitrate solution (mentioned above) and Na2CO3(AR) solution (1 mol·L-1) was dropwise added into the above suspension. The suspension was stirred by a magnetic stirrer and its pH was always maintained at 7 during the preparation process. The following steps were similar with Section 2.1.1. The final sample was denoted as Co-CZS.

    2.1.3 Reverse precipitation method

    A given amount of Na2CO3(AR) solution (1 mol·L-1) was poured into a silica gel suspension (10.0 g silica gel (Sigma-Aldrich, 99.9%)) was suspended in 200 mL deionized water).The resultant mixture was heated to 70 °C. The mixed nitrite solution (mentioned in Section 2.1.1) was then dropped into this mixture. Afterwards, Na2CO3(1 mol·L-1) solution was added to the suspension quickly to adjust the pH to 7. The following steps were similar with Section 2.1.1 and the achieved sample was denoted as Re-CZS.

    2.2 Catalyst characterization

    N2physical adsorption/desorption was carried out on a 3H-2000PS2 instrument. Briefly, after being degassed for 4 h at 150 °C, the sample was characterized at liquid nitrogen temperature. The specific surface area, average pore size and total pore volume were obtained by the B.E.T method and Barrett-Joyner-Halenda (BJH) model, respectively.

    Wide range X-ray diffraction (XRD) pattern was collected from a Rigaku D/Max2500 V diffractometer equipped with Kαradiation of Cu source (λ = 0.154056 nm). All the XRD patterns were scanned from 10° to 80° at a speed of 8 (°)·min-1.

    Temperature-programming desorption (TPD) was performed on a Micromeritics AutoChem 2920 system. For example, 40 mg sample was reduced by 10% H2/Ar gas flow at 250 °C (heating rate 10 °C·min-1) for 2 h. After cooling down to 50 °C under Ar flow, the sample was treated with 10% H2/Ar (10% CO/He or 10% CO2/He) for 30 min. Then the sample was flushed with Ar again to sweep off the physically adsorbed H2(CO or CO2).Finally, the system was heated to 800 °C and the H2(CO or CO2)desorption signal was monitored using a TCD detector. The operation of CO-TPD and CO2-TPD was similar with H2-TPD.

    Temperature-programming reduction (TPR) was also carried out on Micromeritics AutoChem 2920 system. The sample(about 40 mg) was placed in a U-shape quartz reactor.Subsequently, the system was heated to 400 °C and kept for 0.5 h under Ar stream to remove adsorbed impurities. After cooling down to 50 °C, 10% H2/Ar (flow rate of 30 mL·min-1) was introduced into the system. Then, the sample was heated to 500 °C (10 °C·min-1) and H2consumption was calculated by TCD detector.

    The dispersion of Cu species was estimated by using the N2O chemisorption method as stated in our previous work19.

    X-ray photoelectron spectroscopy (XPS) and X-ray excited Auger spectra (XAES) were recorded on an ESCALab220i-XL photoelectron spectrometer with monochromatic Al KαX-ray source (300 W). The C 1s spectral line (284.8 eV) was selected as the reference to correct the static charge accumulation.

    Fourier Transform Infrared Reflection spectroscopy (FT-IR)were recorded on a BRUKER TENSORII spectrometer,equipped with an electromagnetic source in the mid-IR region(4000-400 cm-1). The samples were diluted with 1% (w) KBr and then measured at room temperature.

    Transmission electron microscopy (TEM) was conducted by utilizing JEOL JEM-2100FMII microscope and operated at an accelerating voltage of 200 kV. Especially, at least 80 Cu particles were selected to estimate the average particle size and the surface average particle size was calculated by Eq. (1):

    dis the average particle size andDiis the diameter of the particle.

    2.3 Catalyst evaluation

    Catalytic reactions were tested on a fixed-bed stainless steel reactor (φ9 mm × l450 mm). Before reaction, about 0.5 g sample granules (20 to 40 mesh) was loaded into the middle of the tube reactor and reduced at 250 °C by 10% H2in N2for 4 h.Subsequently, the premixed reaction gas (consisted of 24% CO2,72% H2and 4% Ar where Ar was acted as internal standard) was flushed into reactor for 45 min and then the system pressure was raised to 3 MPa under 50 °C. Finally, the system was heated to 250 °C to evaluate its catalytic performance. The products were analyzed by an on-line gas chromatograph (Panna A91)equipped with a thermal conductivity detector (TCD) and a flame ionized detector (FID).

    The CO2conversion (denoted asX(CO2)) was calculated according to an internal standard method (4% Ar as an internal standard), assuming that the amount of Ar remained constant in the reaction process. The equation as follow:

    3 Results and discussion

    3.1 Metal-support interaction

    TPR analysis were employed to check the metal-support interaction and reducibility of Cu species on the three catalysts(Fig. 1). The main reduction peaks appeared between 240-280 °C illustrating well dispersed Cu species on all the samples20.It is generally considered that higher reduction temperature of CuO might originate from the stronger metal-support interaction and/or lager particle size (poor dispersion of Cu species).

    Fig. 1 TPR profiles of the CuZn/SiO2 catalysts prepared with different methods.

    As listed in Table 1, the H2consumption of Re-CZS, Co-CZS and Nor-CZS catalysts was 1.64, 1.57 and 1.46 mmol·g-1,respectively. The higher hydrogen consumption was related with the more reducible Cu species existing on the catalyst due to the higher dispersion of Cu species. On the other hand, higher reduction temperature was reasonably attributed to the stronger metal-support interaction rather than lager CuO particles. It is thus believed that the Re-CZS catalyst possessed the strongest metal-support interaction while Nor-CZS catalyst might possess the weakest metal-support interaction. Furthermore, the Co-CZS sample showed two reduction peaks suggesting higher heterogeneity of Cu species (various particles size) which would be testified later (Section 3.2).

    The XPS spectrum of Cu 2p(Fig. S1, in Supporting Information, the same below) revealed the distinct chemical environments of the Cu species. The emergence of shake-up satellite peaks at 941.6-944.9 eV unveiled that the Cu species in the fresh samples mainly existed in the form of CuO21. All the Cu 2p3/2signals consisted of two overlapped peaks and their core level signals were deconvoluted into two individual peaks (Fig.2 and Table 2). The peak at 935.1-935.6 eV is usually attributed to the Cu species with stronger interaction with support matrix,and the latter peak (from 933.3 to 933.7 eV) might be ascribed to Cu species with the weaker metal-support interaction22. The characterization results convincingly validated that the metalsupport interaction was successfully altered by the precipitation sequence.

    Fig. 2 XPS spectra of Cu 2p3/2 region of various fresh CuZnO/SiO2catalysts.

    As listed in Table 2, Cu species in the form of both strong metal-support interaction and weaker metal-support interaction were also observed in three catalysts. However, the Re-CZS catalyst possessed the most Cu species (~78%) with strong metal-support interaction, closely followed by Co-CZS (~73%).In contrast, the Nor-CZS contained the most Cu species (~60%)with weaker metal-support interaction. The significant difference in the fraction of Cu species with a strong metalsupport interaction indicated that three catalysts possessed different strength of metal-support interaction. By combining theH2-TPR and XPS results, it could be proposed that the Re-CZS catalyst provided more Cu species with strong metal-support interaction than Nor-CZS catalyst.

    Table 1 Chemical properties of various CuZnO/SiO2 catalysts.

    Table 2 XPS results of Cu 2p3/2 region of various fresh CuZnO/SiO2 catalysts.

    3.2 Textural properties

    The N2-physisorption isotherms for all the catalysts are shown in Fig. 3, in which isotherm of silica gel was also included for comparison. Obviously, the isotherm was of type IV and exhibited a H1 hysteresis loop for silica gel support illustrating that the existence of abundant cylindrical channels on the support. Meanwhile, the high similarity of all isotherms for four samples (including silica gel) indicated that the textures of support were almost preserved after the loading of Cu species23.

    As listed in Table 3, after loading metal, the BET surface area and pore volume of all catalysts decreased in the following order:Nor-CZS > Co-CZS > Re-CZS. It was noted that the micropore of Co-CZS and Re-CZS samples was not detected, indicating the metal species were mainly distributed on the external-surface of SiO2support and then the micropore was blocked by metal particles. Interestingly, the Nor-CZS catalyst displayed the lowest BET surface area and the minimum pore volume and average pore size.

    XRD patterns are shown in Fig. 4. The presence of weak and broaden diffraction peaks at 35.6° and 38.9° implied that most of the Cu species on all the calcined samples were in the form of well dispersed CuO. The crystallite sizes of CuO in the three catalysts displayed in a descending order: Co-CZS (9.1 nm) >Nor-CZS (7.8 nm) > Re-CZS (n.d.) (n.d. meaning diffraction peaks on Re-CZS were too weak to calculate the CuO crystallite sizes according to the Scherrer formula). As a complementary characterization for XRD, N2O chemisorption results are also listed in Table 1. The dispersion of Cu was 18.5% (Re-CZS),16.1% (Co-CZS) and 12.2% (Nor-CZS), respectively. However,the dispersion of Cu particles determined from the N2O chemisorption result was not in full accord with the XRD results.This phenomenon might be attributed to the existence of trace amount of lager CuO (monitored by XRD) on the Co-CZS catalyst19,23, while the less dispersion of Cu determined by N2O chemisorptions on Nor-CZS might also originate from its relatively weak metal-support interaction.

    Fig. 3 N2-physisorption isotherms and pore size distribution of various CuZn/SiO2 catalysts.

    Fig. 4 XRD patterns of various CuZn/SiO2 catalysts.

    Table 3 Textural properties of silica gel and as-calcined catalysts prepared by different methods

    To further illustrate the above conjectures, the representative TEM micrographs and size distribution for three different samples are shown in Fig. 5 and Table 1. The crystallite sizes of CuO in these three catalysts displayed in a descending order: Co-CZS (10.5 nm) > Nor-CZS (9.8 nm) > Re-CZS (8.5 nm).Obviously, partial agglomeration of Cu particles occurred on the support surface for the Co-CZScatalyst. Taking XRD along with N2O chemisorption results into consideration, it could be concluded that the CuZnO/SiO2catalysts with different metalsupport interaction could be modulated through varying the precipitation subsequence24.

    Fig. 5 TEM micrographs and size distribution for fresh (a, d) Nor-CZS catalyst, (b, e) Co-CZS catalyst, (c, f) Re-CZS catalyst.

    To further exclude the formation of Cu phyllosilicate, FT-IR analysis was carried out (Fig. 6). The characteristic bands at 800 cm-1and 1118 cm-1are ascribed to υSiOof different vibration modes of SiO223,25-27. Complete decomposition of carbonates was confirmed by the absence of 1430-1450 cm-1bands in all calcined samples28,29. Particularly, the characteristic δOHband at 670 cm-1was not detected, indicating the absence of Cu phyllosilicate in all the samples27,30.

    Fig. 6 FT-IR spectra of various CuZn/SiO2 catalysts.

    Taken together, the Cu species were well dispersed on all fresh catalysts in the form of CuO regardless of the preparation method. The absence of copper phyllosilicate in all the catalysts elucidated that their notable difference in the metal-support interaction possibly originated from the distinction of the interaction between Cu and ZnO, instead of Cu and SiO2, which was significantly impacted by metal loading process. The stronger metal-support interaction between Cu and ZnO might lead to a higher dispersion of Cu species31,32.

    3.3 Catalysis

    3.3.1 Catalytic performance

    The steady-state activities of the catalysts were measured in a fixed-bed reactor to investigate the relationship between metalsupport interaction and activity of CO2hydrogenation to methanol. It is generally considered that catalytic activity of CO2hydrogenation to methanol is related to the dispersion of Cu species. As described above, the Re-CZS catalyst was supposed to have the best catalytic activity while the Co-CZS catalyst might possess secondary catalytic activity and the Nor-CZS catalyst ought to exhibit the poorest catalytic activity. As expected, the Re-CZS catalyst exhibited the highest activity with 12.4% CO2conversion, followed by the Co-CZS catalyst(12.1%) and then the Nor-CZS catalyst (9.8%) (Fig. S2A and Table 4). The turnover frequency (TOF) values were also calculated with the assumption that each surface Cu atom was an active site (Table 4). An opposite tendency between CO2conversion rate and TOF values was observed due to the small size of Cu particles33,34. The Nor-CZS catalyst exhibited slightly higher TOF value than the Co-CZS sample, demonstrating that the existence of small amount of large bulk CuO had negligible impact on the Cu intrinsic activity. Since, under the current synthesis condition, CO2was mainly involved in two parallel reactions as follows35-37:

    Table 4 The initial CO2 conversion rate, methanol selectivity and methanol productivity (PMeOH).

    The reaction conditions for methanol synthesis were then assessed. As shown in Fig. 7, the Co-CZS catalyst displayed thebest reaction activity under low reaction pressure, while the best reaction activity was obtained over the Re-CZS catalyst with increasing the pressure. However, the former possessed the better methanol selectivity compared with later consistently.

    Fig. 7 Effect of reaction temperature on CO2 conversion (A) and MeOH selectivity (B) and effect of reaction pressure on CO2 conversion (C) and MeOH selectivity (D).

    On the other hand, methanol synthesis was always accompanied by intense exothermic process and accordingly restrained when increasing temperature, while RWGS reaction would be facilitated due to its endothermic process. For this reason, the enhancement of CO2conversion rate accompanied with a decline of methanol selectivity was observed throughout the temperature-rising process. Similar with the former results,the Nor-CZS catalyst also exhibited the highest methanol selectivity and the Re-CZS catalyst possessed the poorest methanol selectivity when the reaction temperature was lower than 270 °C. However, an interesting phenomenon was found when the reaction temperature increased to 290 °C, where the highest methanol selectivity over the Re-CZS catalyst, Nor-CZS and Co-CZS catalysts displayed similar methanol selectivity.These experimental results illustrated that reaction temperature showed great effect on catalytic behavior in comparison to the effect of the reaction pressure. Namely, strong metal-support interaction would improve the dispersion of Cu species and further promote catalytic activity, however, it led to a negative influence on methanol synthesis.

    3.3.2 Catalytic stability

    It was recognized that the catalytic deactivation could be significantly suppressed by the enhancement of metal-support interaction. To compare the relative rate of deactivation, catalytic stability for CO2hydrogenation are evaluated (Fig. 8). Clearly,catalytic activity dropped rapidly during the initial stage of reaction for all catalysts. Especially for the Nor-CZS and Co-CZS catalysts, they suffered from the most severe catalytic deactivation and the reduction of CO2conversion rate(normalized) was more than 20% (22.3%) in the initial 400 min.In contrast, the Re-CZS catalyst displayed better catalytic stability in the initial 400 min and its CO2conversion(normalized) reduced by 15.0%. The stability of three catalysts decreased in the following sequence: Re-CZS > Co-CZS > Nor-CZS. As mentioned above, CO2was involved in two parallel reactions under the methanol synthesis conditions. Therefore,hot spots might be formed on the catalyst due to the high methanol synthesis rate. The higher methanol selectivity would give rise to the severe sintering of Cu species through particle migration and coalescence leading to a dramatic particle growth and significant decrease of Cu surface area, although the reaction temperature was far below the Tammann temperature of Cu species38. Moreover, as mentioned in our previous work19, the existence of large CuO particles could also accelerate particles growth through Ostwald ripening process, in which the growth of larger particles was at the expense of smaller particles. It was reasonable to propose that the similar catalytic stability of Nor-CZS and Co-CZS catalyst at the initial reaction period resulted from higher methanol synthesis rate and the existence of bulk CuO particles for Co-CZS catalyst. With time on stream, the Ostwald ripening was restrained by the vanishing Cu particles meanwhile particle migration and coalescence was also retarded by the decline of methanol yield and relatively stronger metalsupport interaction. Accordingly, the Co-CZS catalyst exhibited the similar deactivation rate with Nor-CZS catalyst at the initial stage and the higher catalytic stability at the medium-late reaction period.

    3.3.3 Structural evolution of catalyst

    As shown in Fig. 8D, the decline trend of CO2conversion was not exactly in line with the decrease process of methanol yield.Especially for the Re-CZS catalyst, in contrast to the maintenance of CO2conversion, the maintenance of the methanol yield was better. After 40 h, the CO2conversion rate decreased by 27.1% (normalized) while its reduction of methanol yield was only about 18.2% (normalized). Obviously,according to Fig. 8C, the enhancement of methanol selectivity over the Re-CZS catalyst during the reaction process was responsible for this phenomenon, while methanol selectivity for the other catalysts exhibited little variation. The Re-CZS catalyst was selected to investigate the cause for this phenomenon. The samples that were calcined, reduced, reacted for 8 h and 40 h,marked as Re-CZS-C, Re-CZS-0, Re-CZS-8 and Re-CZS-40,were characterized with XPS, H2-TPD, CO-TPD and CO2-TPD in detail.

    Fig. 8 Catalytic performance for all catalysts, (A) normalized CO2 conversion, (B) normalized methanol yield, (C) methanol selectivity,(D) deactivation ratio of CO2 conversion and methanol yield.

    As revealed by the XPS results (Fig. S3 and Table S1), the reduction process led to a dramatic decline of Cu content and Cu/(Cu + Zn) ratio (Table S1) on the catalyst’s surface,meanwhile the Zn content on its surface increased slightly. This finding was in good accordance with the results reported by other groups: a part of Zn species migrated from catalyst’s bulk phase to Cu species’ surface owing to strong metal-support interaction32. As a result, partial Cu species on catalyst surface was overlapped by ZnO leading to sample structural restruction after activation process39.

    On the other hand, the H2-TPD results are shown in Fig. S4C and Table S2, reminding that twice reduction process generated insignificant impact on H2adsorption property. Generally, the peak 1, locating at lower temperature, was assigned to desorption of hydrogen adsorbing on Cu surface40, while the broader signal(peak 2), ranging from 300 °C to 650 °C, corresponded to the desorption of strongly adsorbing hydrogen from the surface of ZnO sites deriving from Cu surface through hydrogen spillover41,42. At the initial reaction stage (500 min), the H2desorption originating from Cu surface sharply decreased suggesting the decline of approachable Cu sites on the catalyst surface. Meanwhile, the amounts of H2desorbing from ZnO sites dramatically enhanced which strongly indicated the increase of ZnO surface area due to the further migration of Zn species from mixed bulk phase as reaction proceeds16. Particularly, the decline of Zn/(Cu + Zn + Si) ratio on the catalyst surface (Table S1) manifested that the excessive Zn species would coalesce on the surface of catalyst forming larger ZnO particles. As reaction time prolonged, the H2-TPD results indicated that the desorbing H2from the ZnO surface significantly decreased with the slight enhancement of desorbing H2quantity from Cu sites (still lower than fresh reduced catalyst). This finding further confirmed that leaching and growth of Zn species coexisted on the catalyst although the former process might be limited with time on stream and the slight increase of desorbing H2quantity from Cu surface might be attributed to migration of Zn species on the surface. Moreover, the Cu/(Cu + Zn) ratio on catalyst’s surface showed limited variation while both of the Cu and Zn content on the surface of Re-CZS catalyst declined indicating particle growth for both of zinc and copper species. Herein, the structure evolution of catalyst was proposed and displayed in Scheme 1.

    Obviously, during the sample activation process, restructure of catalyst occurred due to the strong metal-support interaction.At the initial reaction stage, the instability of the catalyst structure led to the growth of Cu particles and the dramatic decline of catalytic activity was accordingly observed. However,the Zn species migrating from bulk phase due to the strong metal-support interaction prevented this process to some extent16,43. With the reaction proceeding, the growth of Cu species was further suppressed and hence the deactivation of catalyst was retarded. Remarkably, leaching and coalescence of Zn species occurred throughout the whole reaction process,which exerted a crucial impact on the methanol synthesis process. From these reaction results (Fig. S2 and Fig. 8C), it was convincible to propose that the catalytic activity (CO2conversion) was principally determined by the exposing Cu species, while the methanol selectivity and productivity was significantly influenced by the leaching of Zn species.

    It was widely acknowledged that there was an intimate synergy between Cu and Zn species, where ZnO acted as direct promoter for C―O bond activation and hydrogen reservoir. In consequence, similar variation trend between the CO2and H2chemisorption results was expected44. The CO2-TPD profiles were shown in Fig. S4A, with their details summarized in Table S2. As expected, similar to the H2-TPR result, the twice reduction process also generated the slight impact on CO2adsorption property and its variation trend further confirmed our hypothesis as proposed in Scheme 1.

    Scheme 1 Catalyst structure evolution process.

    Scheme 2 The reaction mechanism of methanol synthesis process.

    To further investigate the relationship between structure evolution of the catalyst and formation of methanol, CO2-TPD results (ranging from 230 °C to 700 °C) at various reaction times were deconvoluted into three Gaussian peaks, as shown in Fig.9, and the relative content and the number of each basic sites were listed in Table 5. Notably, because of relatively high reaction temperature (250 °C), the CO2desorption peak at the lower temperature (about 100 °C) was considered to have a limited contribution to the CO2activation and therefore it was convincible to consider that the catalytic performance corresponded to later peak. Generally, different desorption temperature of the three peaks indicated the existence of different CO2adsorbing species on the catalyst. In other words,it’s logical to deduce that there should be three different CO2adsorption sites existed on the catalyst surface.

    Fig. 9 CO2-TPD results for Re-CZS catalyst with different reaction time.

    Table 5 Relative contents of deconvoluted peaks from CO2-TPD.

    The results illustrated that migration of ZnO could not only improve the adsorption capacity of H2but also alter the number and property of CO2adsorption sites which played a crucial role in the CO2hydrogenation. As reported45, the weakly and medially basic sites (peak 2) were corresponded to metal-oxygen pairs (such as isolated ZnO) with different adsorption manners in which the RWGS reaction mainly occurred, while the strongly basic sites (peak 3) were assigned to the low coordination oxygen atoms which greatly facilitated formation of methanol.The results indicated that the relative content and the number of weakly and medially basic site decreased with time on stream,while strongly basic sites displayed a contrary tendency indicating the transformation of basic sites during the reaction process. As a result, the improvement of methanol selectivity was obtained with time on stream. It was also noted that the enhancement of strongly basic sties owing to the migration of Zn species suggested that more Cu/ZnO interface could facilitate formation of low coordination oxygen atoms.

    Eventually, CO-TPD has also been carried out to further clarify the impact of ZnO migration process. Different from the H2-TPD and CO2-TPD results, the CO-TPD results (Fig. S4B)clearly manifested that the capacity for the CO adsorption in the temperature range of 200 to 700 °C was significantly enhanced as the reaction progress. Therefore, it was plausible to propose that the adsorption sites for CO2and CO was definitely different and the CO conversion (deriving from RWGS) to methanol might be further facilitated owing to the improvement of CO adsorption capacity.

    Conclusively, the migration of ZnO from the bulk catalyst owing to the strong-metal support interaction could not only improve the adsorption capacity of H2which could facilitate methanol synthesis process, but alter the property of CO2adsorption sites which was considered to greatly influence the CO2hydrogenation performance of catalyst46. However, the excessive Zn species would accelerate the formation of slightly lager ZnO particles resulting in a negative impact on CO2hydrogenation process and a positive impact on CO hydrogenation process. Therefore, it’s rational to infer that there should exist a balance between leaching and migration of Zn species, which was greatly affected by the metal-support interaction.

    Based on the above investigation, a reaction mechanism was proposed (Scheme 2). Initially, the H2dissociates on the Cuδ+site and then spillovers to the Cu/ZnO interface and the ZnO surface through route Haand Hb, respectively. Then, the H* (generated by spillover from Cuδ+site) would react with the different adsorbed CO2. Subsequently, methanol and CO were produced on different active sites. Particularly, the majority of CO generated from RWGS reaction would desorb from catalyst surface while the others might furtherreact with the H* to form methanol.

    4 Conclusions

    In summary, three Cu/ZnO-SiO2catalysts with different metal-support interaction could be modulated through varying the precipitation sequence. The role of Cu-ZnO interaction on the catalytic activity of CO2hydrogenation to methanol was investigated by a combination of characterization and reaction.It is revealed that intimate interaction between the Cu and Zn species promotes the dispersion of Cu species, which was beneficial to the CO2activation. Stronger metal-support interaction (MSI) was conducive to improve the activity and stability of the catalyst. The migration of ZnO from bulk catalyst induced by the strong metal-support interaction (MSI) not only promoted the adsorption and activation of H2and CO2, thereby facilitating the activation efficiency of the reactants, but also changed the reaction pathway of the CO2hydrogenation to some extent. We believe that this work is helpful for understanding of the metal-support interaction in Cu-based catalysts, and also provide guidance for the rational and optimized design of efficient catalysts.

    Supporting information: available free of charge via the internet at http://www.whxb.pku.edu.cn.

    亚洲综合精品二区| 99精国产麻豆久久婷婷| 精品少妇黑人巨大在线播放| 亚洲av欧美aⅴ国产| 久久久久视频综合| 在现免费观看毛片| 亚洲少妇的诱惑av| 成人免费观看视频高清| av免费观看日本| 国产成人啪精品午夜网站| 高清欧美精品videossex| 黄网站色视频无遮挡免费观看| 精品国产一区二区三区四区第35| 99国产综合亚洲精品| 国产欧美日韩综合在线一区二区| 国产av国产精品国产| 青春草国产在线视频| 男女无遮挡免费网站观看| 午夜福利在线免费观看网站| 亚洲av成人精品一二三区| 久久综合国产亚洲精品| 999精品在线视频| 亚洲成人国产一区在线观看 | 成人亚洲欧美一区二区av| 国产一区二区三区av在线| 成人漫画全彩无遮挡| 97精品久久久久久久久久精品| 久久精品熟女亚洲av麻豆精品| 欧美激情高清一区二区三区 | 一区福利在线观看| 亚洲一区二区三区欧美精品| 久久影院123| 观看美女的网站| 韩国av在线不卡| 人妻 亚洲 视频| 19禁男女啪啪无遮挡网站| 啦啦啦 在线观看视频| 精品少妇久久久久久888优播| 亚洲成色77777| 国产精品嫩草影院av在线观看| 一本色道久久久久久精品综合| 久久这里只有精品19| 国产精品秋霞免费鲁丝片| 国产97色在线日韩免费| 一级毛片电影观看| 亚洲精品av麻豆狂野| 亚洲精品中文字幕在线视频| 五月开心婷婷网| av福利片在线| 免费观看性生交大片5| 欧美亚洲日本最大视频资源| 国产一区二区三区综合在线观看| 精品一区二区三区四区五区乱码 | 久久久久久久久免费视频了| 男人舔女人的私密视频| 亚洲人成77777在线视频| 午夜老司机福利片| 国产在视频线精品| 无遮挡黄片免费观看| 一级毛片黄色毛片免费观看视频| av又黄又爽大尺度在线免费看| 中文字幕精品免费在线观看视频| 久久婷婷青草| 欧美亚洲 丝袜 人妻 在线| 国产人伦9x9x在线观看| 悠悠久久av| 国产探花极品一区二区| 精品国产乱码久久久久久小说| 一区二区三区四区激情视频| 人人妻,人人澡人人爽秒播 | 久久精品亚洲av国产电影网| 日日摸夜夜添夜夜爱| 中文字幕制服av| 岛国毛片在线播放| 亚洲av成人精品一二三区| 亚洲国产欧美网| 国产乱人偷精品视频| 国产av精品麻豆| 成人国产麻豆网| 好男人视频免费观看在线| 伊人久久国产一区二区| 在线看a的网站| 国产亚洲欧美精品永久| 99热全是精品| 黄色视频不卡| 各种免费的搞黄视频| 在现免费观看毛片| av视频免费观看在线观看| 亚洲精品日韩在线中文字幕| 精品少妇久久久久久888优播| 女的被弄到高潮叫床怎么办| 99国产综合亚洲精品| 成年女人毛片免费观看观看9 | 另类精品久久| 成年人免费黄色播放视频| 一区二区三区精品91| 91aial.com中文字幕在线观看| 哪个播放器可以免费观看大片| 日本wwww免费看| 两性夫妻黄色片| 99热网站在线观看| 亚洲综合色网址| 中国国产av一级| 国语对白做爰xxxⅹ性视频网站| 亚洲精品成人av观看孕妇| 久久久久久人人人人人| 精品人妻一区二区三区麻豆| 1024香蕉在线观看| 女人久久www免费人成看片| 国产黄色免费在线视频| 日日撸夜夜添| 午夜免费鲁丝| 久热爱精品视频在线9| av在线老鸭窝| 成人亚洲精品一区在线观看| 国产男女内射视频| 丰满饥渴人妻一区二区三| 最近手机中文字幕大全| 精品一品国产午夜福利视频| 欧美亚洲 丝袜 人妻 在线| 亚洲精品久久午夜乱码| 天天躁狠狠躁夜夜躁狠狠躁| 亚洲av中文av极速乱| 久久人人爽av亚洲精品天堂| 高清在线视频一区二区三区| 一级,二级,三级黄色视频| 亚洲国产精品一区三区| 嫩草影视91久久| 欧美激情高清一区二区三区 | 精品视频人人做人人爽| 制服诱惑二区| 日韩免费高清中文字幕av| 男人添女人高潮全过程视频| 午夜福利网站1000一区二区三区| 夫妻午夜视频| 18禁观看日本| 欧美激情高清一区二区三区 | 亚洲精品美女久久av网站| 精品国产乱码久久久久久小说| 日韩欧美精品免费久久| 久久毛片免费看一区二区三区| 又大又爽又粗| 色播在线永久视频| 考比视频在线观看| 亚洲欧洲国产日韩| 亚洲欧美一区二区三区国产| 国产精品.久久久| 国产97色在线日韩免费| 青春草国产在线视频| 大香蕉久久网| 亚洲精品乱久久久久久| 亚洲成人一二三区av| 国产高清不卡午夜福利| 国产人伦9x9x在线观看| 十八禁高潮呻吟视频| 亚洲精品aⅴ在线观看| 成人漫画全彩无遮挡| 自线自在国产av| 制服丝袜香蕉在线| 欧美精品av麻豆av| 丝袜脚勾引网站| 黄网站色视频无遮挡免费观看| 人人妻人人澡人人看| 精品久久蜜臀av无| 校园人妻丝袜中文字幕| 曰老女人黄片| 无遮挡黄片免费观看| 久久久久久久久久久免费av| 青草久久国产| 中文精品一卡2卡3卡4更新| 精品卡一卡二卡四卡免费| 久久久久久久大尺度免费视频| kizo精华| 亚洲国产欧美一区二区综合| 精品久久蜜臀av无| 一本久久精品| av线在线观看网站| 九草在线视频观看| 91aial.com中文字幕在线观看| 国产一区二区 视频在线| av女优亚洲男人天堂| 欧美变态另类bdsm刘玥| 亚洲欧美成人综合另类久久久| 国产片特级美女逼逼视频| 91精品三级在线观看| 国产麻豆69| 黄色视频在线播放观看不卡| 女人久久www免费人成看片| 成人三级做爰电影| 久久精品国产a三级三级三级| 最近最新中文字幕大全免费视频 | 亚洲欧美清纯卡通| 亚洲成人国产一区在线观看 | 亚洲综合精品二区| 日韩,欧美,国产一区二区三区| 桃花免费在线播放| 建设人人有责人人尽责人人享有的| 亚洲成色77777| 国产精品 欧美亚洲| 18禁动态无遮挡网站| 男女免费视频国产| 大片免费播放器 马上看| avwww免费| 亚洲一卡2卡3卡4卡5卡精品中文| 侵犯人妻中文字幕一二三四区| 久久精品人人爽人人爽视色| 丰满乱子伦码专区| 国产一区有黄有色的免费视频| 亚洲美女黄色视频免费看| 又黄又粗又硬又大视频| 国产毛片在线视频| 国产男女内射视频| 国产野战对白在线观看| 日韩大码丰满熟妇| 国产精品嫩草影院av在线观看| 1024香蕉在线观看| 国产亚洲欧美精品永久| 亚洲少妇的诱惑av| 婷婷色综合大香蕉| 国产精品嫩草影院av在线观看| 国产一区二区三区综合在线观看| 精品一区在线观看国产| 天天躁狠狠躁夜夜躁狠狠躁| 日韩伦理黄色片| 欧美日韩av久久| videosex国产| 欧美精品av麻豆av| 国产精品香港三级国产av潘金莲 | 国产免费视频播放在线视频| 1024香蕉在线观看| 18禁裸乳无遮挡动漫免费视频| 亚洲精品在线美女| 美女大奶头黄色视频| 毛片一级片免费看久久久久| 成人午夜精彩视频在线观看| 18禁裸乳无遮挡动漫免费视频| 亚洲精品国产区一区二| 久久天躁狠狠躁夜夜2o2o | 日日啪夜夜爽| 免费在线观看黄色视频的| 一二三四在线观看免费中文在| 亚洲人成77777在线视频| 国产精品一区二区在线不卡| 日韩电影二区| 各种免费的搞黄视频| 飞空精品影院首页| av在线观看视频网站免费| 婷婷色综合www| 国产探花极品一区二区| 国产人伦9x9x在线观看| h视频一区二区三区| 菩萨蛮人人尽说江南好唐韦庄| 亚洲三区欧美一区| 国产免费现黄频在线看| 成人国语在线视频| 日本欧美国产在线视频| 国产乱人偷精品视频| 久久久国产精品麻豆| 免费高清在线观看视频在线观看| 免费久久久久久久精品成人欧美视频| 下体分泌物呈黄色| 热re99久久精品国产66热6| 亚洲精品久久成人aⅴ小说| 欧美亚洲 丝袜 人妻 在线| 久久影院123| 国产精品久久久久久久久免| 伦理电影大哥的女人| 最新在线观看一区二区三区 | av天堂久久9| 日韩中文字幕欧美一区二区 | 你懂的网址亚洲精品在线观看| 欧美日韩亚洲国产一区二区在线观看 | av在线app专区| av.在线天堂| 午夜久久久在线观看| 国产无遮挡羞羞视频在线观看| 777久久人妻少妇嫩草av网站| 国产精品免费视频内射| 日韩电影二区| 色网站视频免费| 精品久久久久久电影网| 王馨瑶露胸无遮挡在线观看| 国产深夜福利视频在线观看| 最近中文字幕2019免费版| 中文精品一卡2卡3卡4更新| 色婷婷久久久亚洲欧美| tube8黄色片| 男的添女的下面高潮视频| av网站在线播放免费| 亚洲欧美中文字幕日韩二区| 一区福利在线观看| 国产精品 国内视频| 成人影院久久| 亚洲欧美激情在线| 深夜精品福利| 亚洲美女视频黄频| 天天躁日日躁夜夜躁夜夜| 日韩电影二区| 午夜av观看不卡| 青春草亚洲视频在线观看| 欧美成人精品欧美一级黄| 亚洲成人av在线免费| 大片电影免费在线观看免费| 亚洲欧美激情在线| videosex国产| 啦啦啦在线观看免费高清www| 国产片特级美女逼逼视频| 深夜精品福利| 亚洲av男天堂| 亚洲欧美精品综合一区二区三区| 在线精品无人区一区二区三| 成人国产av品久久久| 人人妻人人爽人人添夜夜欢视频| 十八禁人妻一区二区| 久久久久久久精品精品| 午夜日韩欧美国产| 国产老妇伦熟女老妇高清| 国产xxxxx性猛交| 亚洲国产欧美一区二区综合| 美女扒开内裤让男人捅视频| 国产精品国产三级国产专区5o| 国产伦理片在线播放av一区| 欧美精品一区二区免费开放| 亚洲,一卡二卡三卡| 久久久久久久国产电影| 蜜桃在线观看..| 日韩伦理黄色片| 国产精品熟女久久久久浪| 尾随美女入室| 在线观看免费午夜福利视频| 99九九在线精品视频| 秋霞伦理黄片| av免费观看日本| 一本大道久久a久久精品| 欧美老熟妇乱子伦牲交| 少妇人妻久久综合中文| 国产老妇伦熟女老妇高清| 99国产精品免费福利视频| 中国三级夫妇交换| 日韩中文字幕欧美一区二区 | 国产在线免费精品| 国产亚洲午夜精品一区二区久久| 中文字幕制服av| 欧美精品人与动牲交sv欧美| 啦啦啦中文免费视频观看日本| 国产亚洲av片在线观看秒播厂| 青草久久国产| a级毛片黄视频| 亚洲中文av在线| 黑人猛操日本美女一级片| 亚洲精品国产区一区二| 免费观看人在逋| 国产精品女同一区二区软件| 亚洲精品一区蜜桃| 麻豆av在线久日| 好男人视频免费观看在线| 国产午夜精品一二区理论片| 亚洲欧洲国产日韩| 9热在线视频观看99| 熟女av电影| 国产欧美日韩综合在线一区二区| 夜夜骑夜夜射夜夜干| 精品一品国产午夜福利视频| 欧美日韩福利视频一区二区| 日韩欧美精品免费久久| 波多野结衣av一区二区av| 在线观看免费日韩欧美大片| 一级毛片我不卡| 亚洲久久久国产精品| 国产精品亚洲av一区麻豆 | 成人毛片60女人毛片免费| 2021少妇久久久久久久久久久| 波野结衣二区三区在线| 欧美乱码精品一区二区三区| 叶爱在线成人免费视频播放| 天天躁日日躁夜夜躁夜夜| 精品国产一区二区三区久久久樱花| 久久韩国三级中文字幕| 日韩欧美一区视频在线观看| 午夜老司机福利片| 老司机在亚洲福利影院| 亚洲,欧美精品.| 国产97色在线日韩免费| 天堂俺去俺来也www色官网| 成人亚洲欧美一区二区av| 男女国产视频网站| 免费黄网站久久成人精品| av在线观看视频网站免费| 日韩中文字幕欧美一区二区 | 两个人看的免费小视频| 欧美黑人欧美精品刺激| 中文字幕av电影在线播放| 国产一区二区三区综合在线观看| 日日爽夜夜爽网站| 亚洲精华国产精华液的使用体验| 久久精品久久久久久噜噜老黄| 人妻人人澡人人爽人人| 夜夜骑夜夜射夜夜干| 日韩精品免费视频一区二区三区| 99香蕉大伊视频| 水蜜桃什么品种好| 久久国产精品大桥未久av| 观看美女的网站| 国产又爽黄色视频| 欧美在线一区亚洲| 国产av国产精品国产| 日本91视频免费播放| 波野结衣二区三区在线| 这个男人来自地球电影免费观看 | 久久精品久久久久久久性| 欧美成人午夜精品| 国产精品av久久久久免费| 啦啦啦在线免费观看视频4| 两个人免费观看高清视频| 成人国产av品久久久| 两个人免费观看高清视频| av一本久久久久| 亚洲国产精品999| 久久青草综合色| 成人亚洲精品一区在线观看| 亚洲国产欧美网| 欧美日韩亚洲综合一区二区三区_| 老司机深夜福利视频在线观看 | 久久国产精品大桥未久av| 最近手机中文字幕大全| 一级片免费观看大全| 免费黄色在线免费观看| 黄片无遮挡物在线观看| 丝瓜视频免费看黄片| 成人国语在线视频| 80岁老熟妇乱子伦牲交| 久久久久久久精品精品| 色网站视频免费| 色婷婷久久久亚洲欧美| 免费高清在线观看视频在线观看| 丝袜在线中文字幕| 女人精品久久久久毛片| 久久久精品免费免费高清| 丰满迷人的少妇在线观看| 欧美日本中文国产一区发布| 国产成人a∨麻豆精品| 中文字幕另类日韩欧美亚洲嫩草| 国产精品99久久99久久久不卡 | 十八禁高潮呻吟视频| xxx大片免费视频| 国产精品国产av在线观看| 成人18禁高潮啪啪吃奶动态图| 日韩,欧美,国产一区二区三区| 欧美 日韩 精品 国产| 亚洲熟女精品中文字幕| 男人舔女人的私密视频| av又黄又爽大尺度在线免费看| 久久久精品免费免费高清| 精品一区二区三区av网在线观看 | 久久热在线av| 久久久国产精品麻豆| 欧美 亚洲 国产 日韩一| 久久99一区二区三区| 欧美成人午夜精品| 亚洲av成人精品一二三区| 天天影视国产精品| 制服人妻中文乱码| 久久鲁丝午夜福利片| 一级毛片我不卡| 欧美精品人与动牲交sv欧美| 欧美亚洲日本最大视频资源| 七月丁香在线播放| 久久久精品免费免费高清| 我的亚洲天堂| 精品国产一区二区三区久久久樱花| 一边摸一边抽搐一进一出视频| 久久99精品国语久久久| 久久久久久人妻| 成年女人毛片免费观看观看9 | 久久久久久久久久久免费av| 国产老妇伦熟女老妇高清| 只有这里有精品99| 亚洲精品一区蜜桃| 夫妻午夜视频| 精品少妇黑人巨大在线播放| 91老司机精品| 人妻一区二区av| svipshipincom国产片| 午夜福利视频在线观看免费| 日本一区二区免费在线视频| 亚洲精品在线美女| 18在线观看网站| 国产亚洲av高清不卡| 母亲3免费完整高清在线观看| 亚洲精品国产av成人精品| videosex国产| 少妇猛男粗大的猛烈进出视频| 不卡视频在线观看欧美| 91老司机精品| 亚洲,欧美,日韩| 午夜免费鲁丝| 大香蕉久久网| 男人爽女人下面视频在线观看| 国产黄频视频在线观看| 伊人久久国产一区二区| svipshipincom国产片| 九草在线视频观看| 成年人午夜在线观看视频| 香蕉国产在线看| 涩涩av久久男人的天堂| 久久久久人妻精品一区果冻| 亚洲人成77777在线视频| 国产 精品1| 欧美日韩一级在线毛片| 亚洲国产看品久久| av在线播放精品| 大话2 男鬼变身卡| 蜜桃国产av成人99| 国产成人欧美在线观看 | 久久天躁狠狠躁夜夜2o2o | 90打野战视频偷拍视频| 水蜜桃什么品种好| 少妇人妻 视频| avwww免费| 亚洲,一卡二卡三卡| 大话2 男鬼变身卡| 亚洲国产欧美日韩在线播放| 成年女人毛片免费观看观看9 | 97精品久久久久久久久久精品| 亚洲av欧美aⅴ国产| 欧美日韩精品网址| 1024视频免费在线观看| 黄色视频在线播放观看不卡| 天天躁夜夜躁狠狠久久av| 久久久久国产精品人妻一区二区| 天天操日日干夜夜撸| 久久精品亚洲熟妇少妇任你| 国产精品.久久久| 中文字幕av电影在线播放| 国产在线视频一区二区| 久久精品久久精品一区二区三区| 国产一区二区三区综合在线观看| 亚洲色图综合在线观看| 大香蕉久久网| 精品卡一卡二卡四卡免费| 久久久国产精品麻豆| 啦啦啦视频在线资源免费观看| 人体艺术视频欧美日本| 欧美成人午夜精品| 一级毛片 在线播放| 熟女av电影| 无限看片的www在线观看| 91国产中文字幕| 精品亚洲成a人片在线观看| 国产亚洲最大av| 亚洲成色77777| 亚洲精品第二区| 亚洲精品视频女| 日日啪夜夜爽| 9色porny在线观看| 欧美激情高清一区二区三区 | 日本色播在线视频| 久久狼人影院| 亚洲成人手机| 欧美日韩成人在线一区二区| 一个人免费看片子| 久久久久久久精品精品| 永久免费av网站大全| 免费黄网站久久成人精品| 久久久精品94久久精品| 国产av精品麻豆| 亚洲成人一二三区av| 午夜激情久久久久久久| 久久久久久久久久久免费av| 一级黄片播放器| 97人妻天天添夜夜摸| 成人国产麻豆网| kizo精华| 不卡av一区二区三区| av福利片在线| 国产精品国产av在线观看| av电影中文网址| 男人操女人黄网站| 日韩一区二区视频免费看| 亚洲国产欧美网| 91国产中文字幕| 日韩 欧美 亚洲 中文字幕| 丁香六月欧美| 丝袜人妻中文字幕| av在线老鸭窝| 中文字幕av电影在线播放| 视频在线观看一区二区三区| 亚洲成人一二三区av| 国产精品免费大片| 色94色欧美一区二区| 一区二区三区激情视频| 久久久久国产一级毛片高清牌| 黄色视频不卡| 国产亚洲av高清不卡| 日韩中文字幕视频在线看片| www.av在线官网国产| 久热爱精品视频在线9| 一本色道久久久久久精品综合| 看免费成人av毛片| 亚洲精品成人av观看孕妇| 精品久久蜜臀av无| 久久久国产精品麻豆| 在线免费观看不下载黄p国产| 日日撸夜夜添| 深夜精品福利| 久久国产亚洲av麻豆专区| 欧美日韩一区二区视频在线观看视频在线| 国产精品久久久久久精品电影小说| 国产欧美日韩综合在线一区二区| 日韩一区二区视频免费看| 欧美日韩视频高清一区二区三区二| 久久精品国产亚洲av涩爱| 夜夜骑夜夜射夜夜干| 又大又黄又爽视频免费| 国产毛片在线视频|