    Brazing of C/C composite and Ti-6Al-4V with graphene strengthened AgCuTi filler:Effects of graphene on wettability,microstructure and mechanical properties

    2018-07-24 09:00:10DuoLIUYnyuSONGYinghoZHOUXioguoSONGWeiFUJiciFENG
    CHINESE JOURNAL OF AERONAUTICS 2018年7期

    Duo LIU,Ynyu SONG,Yingho ZHOU,Xioguo SONG,*,Wei FU,Jici FENG

    aState Key Laboratory of Advanced Welding and Joining,Harbin Institute of Technology,Harbin 150001,China

    bShandong Provincial Key Laboratory of Special Welding Technology,Harbin Institute of Technology at Weihai,Weihai 264209,China

    KEYWORDS Brazing;Graphene nanosheets;Mechanical properties;Microstructure;Wetting

    Abstract Graphene nanosheets(GNSs)strengthened AgCuTi composite filler(AgCuTiG)was used to braze C/C composite and Ti-6Al-4V.The effects of GNSs on the wettability of AgCuTiG filler on the C/C composite surface and the interfacial microstructure and mechanical properties of brazed joints were investigated.The results indicate that the addition of GNSs reduced the wettability of AgCuTiG.The interfacial microstructure of brazed joints evolved with the addition of GNSs,where Ti3Cu4and TiCu4were converted to TiCu and the thickness of the reaction layer adjacent to the base material decreased.The maximum shear strength of joints brazed at 0.3wt%GNSs was 23.3 MPa(880°C/10 min).Further adding GNSs deteriorated the shear strength of the joints.Fracture of the joints occurred in the C/C composite substrate and the TiC layer adjacent to C/C composite.

    1.Introduction

    As a promising high-temperature structure material,carbon fiber reinforced carbon matrix composite(C/C composite)possesses low coefficient of thermal expansion(CTE),good anti-fatigue ability,high thermal conductivity and hightemperature mechanical properties,and is widely utilized in aeronautics and space industries.1–3To enhance their potential for practical applications in aerospace components,it is necessary to join C/C composite to other materials.Ti-6Al-4V alloy(TC4)can be widely applied in aerospace industries owing to its excellent mechanical properties such as high specific strength and strong corrosion resistance.4,5As part of a proposed nozzle component,the bonding of C/C composite and TC4 can greatly decrease the weight and increase the efficiency of rocket engines.6

    Among different kinds of joining methods,brazing is a common method to join C/C composite to metals because of its strongadaptabilityandlowcost.However,thewettabilityof filler metals on composite surface was a problem in brazing C/C composite to metals.7–11Previous research primarily focused on the effects of active elements on the wettability of filler alloy.Singh et al.investigated the effect of Ti content in different filler systems on the wettability on C/C composite surface.12The wettability of Pd-35Co,Pd-40Ni,63Ag-35.3Cu-1.75Ti and 68.8Ag-26.7Cu-4.5Ti fillers on C/C composite was reported by Asthana et al.13Several studies reported the wetting process of f i llers on C/C composite.In addition,high residual stress occurred at the brazed joints due to the diversity in elasticity modulus and CTE between C/C composite and metals.Therefore,composite filler,which is prepared by adding reinforcement particles with a high elasticity modulus and a low CTE into traditional active fillers to improve the strength of brazed joints,has attracted great interest in recent years.Lin et al.14used TiB2reinforced Cu-Ni composite filler to join C/C composite to TiBw/TC4,and the shear strength of brazed joints was improved.The use of micro-SiC particles decreased thethicknessofreactionlayersnearC/Ccompositeandreduced the mismatch of CTEs between C/C composite and TC4,which ledtoareductionoftheresidualstressofthejoints.15Zhouetal.analyzed the strengthening mechanism of nano-Al2O3particles in improving the mechanical properties of brazed joints.9Graphene,as a perfect two-dimensionalmaterialof sp2-bonded carbon atoms,has attracted wide attention owing to its excellent comprehensive properties including high Young’s modulus,fracture strength,thermal conductivity and specific surface area.16,17In addition,GNSs composed of a few graphene layers possess properties similar to those of single-layer graphene,and are more prone to produce and handle.18GNSshavebeenproposedforpotentialapplicationsinthe nanoelectronics field,19and applied to improve the mechanical properties of materials.20

    Therefore,GNSs reinforced AgCuTi composite filler was selected to join C/C composite to TC4 alloy in this study.The wettability of AgCuTi filler with different GNSs contents on C/C composite was studied.The effects of the GNSs content on the interfacial microstructure and mechanical properties of brazed joints were investigated.

    2.Experimental procedure

    The substrate materials used in this study were C/C composite and TC4 alloy.C/C composite was cut into specimens with sizes of 20 mm×20 mm×5 mm and 5 mm×5 mm×5 mm for wetting and brazing experiments using a diamond cutting machine.TC4 alloy was cut into specimens with a size of 20 mm×10 mm×3 mm by a wire electric discharge machine.AgCuTiGfiller was prepared by adding GNSs and titanium powder (4.5wt%) into AgCu eutectic powder filler(Ag-26.7 wt%Cu).The contents of GNSs in the composite filler were 0wt%,0.1wt%,0.3wt%,0.5wt%and 0.8wt%,respectively.Then the mixture was milled for 4 hours with a speed of 150 r/min using a QM-SB planetary ball mill.The composite filler powder was pressed into a?6 mm×4 mm cylinder under a pressure of 3 MPa.All the specimens were polished and ultrasonic cleaned in acetone for 10 min.

    The wetting experiments were conducted through the sessile drop method,which were carried out in a high-temperature wetting measuring device under a vacuum of 5×10-4Pa.The processed C/C composite substrate was placed on the sample stage and adjusted to a horizontal position.AgCuTiGwas placed at the center of C/C composite.To ensure temperature consistency in the furnace,the sample assembly was firstly heated to 750 °C at a rate of 20 °C/min and held for 10 min.Then it was heated to 880 °C at a rate of 5 °C/min and held for a period of time.Finally,the assembly was cooled down to 400 °C at a rate of 5 °C/min and then furnace-cooled down to the room temperature.The brazing experiments were performed in avacuum furnaceunderavacuum of 3×10-3Pa.AgCuTiGfiller was placed between C/C composite and TC4.The process parameters were similar to those of the wetting experiments.

    The polished cross-sections of wetting samples and C/C composite/TC4 brazed joints were examined with a field emission scanning electron microscope(SEM)equipped with an energy dispersive spectrometer(EDS)to observe the interfacial microstructure morphology.The phase compositions of the interface was identified by X-ray diffraction(XRD).The shear strength of the brazed joints was tested with an Instron 5967 universal material testing machine.A schematic diagram of the shear test is shown in Fig.1.The specimens were loaded by the testing machine with a constant displacement rate of 0.5 mm/min.At least 4 specimens brazed at the same brazing parameters were tested to obtain an average shear strength.The fracture surface was observed using SEM and EDS.

    3.Results and discussion

    3.1.Effects of GNSs on the wettability of AgCuTiG filler

    Fig.1 Schematic diagram of shear test of C/C composite/AgCuTiG/TC4 joints.

    Fig.2 Variations of drop height and contact angle with different GNSs contents.

    Fig.2(a)shows the variation of the drop height with time for different GNSs contents during the isothermal holding at temperatureT=880°C.It can be seen from the image that the content of GNSs had a great effect on the wettability of AgCuTi filler on the C/C composite substrate.The contact angle of 7.71°and the drop height of 0.65 mm show excellent wetting between AgCuTi filler and C/C composite,as displayed in Fig.2(b).When the content of GNSs was more than 0.3wt%,the contact angle and drop height increased obviously,so the wettability of composite filler reduced.Depending on the variations of the contact angle and drop height,the wetting process of AgCuTiGfiller can be divided into three stages.(1)Rapid decrease stage(timet=0–600 s).The height of droplet decreased obviously with the increase of the holding time due to the fast wetting and spreading rate,and the initial drop height ranged from 1.25 mm to 1.95 mm when adding GNSs from 0wt%to 0.8wt%.(2)Slow decrease stage(600–2000 s).The height of droplet decreased slowly with increasing the holding time,and the slow decrease stage can last for a long period of time when the content of GNSs was below 0.3wt%.(3)Equilibrium stage(2000–4000 s).The wetting process tended to be a balance when it reached 2000 s.The f i nal drop height of 0.3–0.7 mm was obtained when the GNSs content was in the range of 0wt%–0.3wt%,indicating good wettability.

    Fig.3 shows the interfacial microstructure of droplet/C/C composite at 880°C for 70 min.Fig.3(a)indicates that four different phases were distributed on the interface.The EDS results were demonstrated in Table 1.The gray phase(spot A)was Cu-based solid solution(Cu(s,s)),and the white phase(spot B)was Ag-based solid solution(Ag(s,s)).TiC(spots C and D)was distributed on the interface adjacent to the C/C composite substrate and in the molten droplet.The black phase(spot E)was GNSs.XRD analysis was performed to further confirm the phases.As presented in Fig.3(b),Ag(s,s)and Cu(s,s)were examined in the droplet without GNSs.The diffraction peaks of TiC appeared at 0.3wt%GNSs,which confirmed that Ti reacted with GNSs to form the TiC phase.When the GNSs content rose up to 0.8wt%,highly-enriched GNSs consumed Ti in the filler alloy,and residual GNSs were detected in the XRD pattern.

    In order to accurately analyze the effect of the GNSs content on the wettability of the composite filler,the interfacial microstructure of droplet/C/C composite is shown in Fig.4.The GNSs content ranged from 0wt%to 0.8wt%.Block Cu(s,s),Ag(s,s)and a thicker TiC layer adjacent to the C/C composite substrate were observed in the droplet/C/C composite interface when using AgCuTi filler without GNSs.With the addition of GNSs,the amount of block solid solution decreased.This may be attributed to the fact thatflaky GNSs impeded the diffusion of elements in filler alloy,therefore,some of these elements were distributed around GNSs.In addition,the thickness of the TiC layer decreased due to the reaction between GNSs and Ti.Residual GNSs after the reaction appeared in the interfacial microstructure at 0.8wt%GNSs.

    3.2.Effects of GNSs on the microstructure of C/C composite/TC4 brazed joints

    The typical interfacial microstructure of the C/C composite/AgCuTi/TC4 joint brazed at 880°C for 10 min is shown in Fig.5(a).It can be seen that the brazed joint mainly consisted of four distinct parts marked by I,II,III and IV.As shown in Table 2,there were much Ti and some Al and V in layer I.Layer II was mainly composed of Cu and Ti,according to the EDS results and phase diagram of the titanium-copper system,it can be inferred that the reaction products from spots B to E were Ti2Cu,TiCu,Ti3Cu4and TiCu4.The white phases in layer III consisted of much Ag and little Cu,so there was Agbased solid solution(Ag(s,s)).Meanwhile,Ti-Cu compounds were distributed on the Ag(s,s)substrate.Layer IV near C/C composite was TiC layer.Similar conclusions were also obtained in Ref.21.Therefore,it can be concluded that the interface structure of the C/C composite/TC4 joint brazed at 880°C for 10 min can be expressed as TC4/diffusion layer/Ti2Cu+TiCu+Ti3Cu4+TiCu4/Ag(s,s)+Ti3Cu4+TiCu4+TiCu/TiC/C/C composite.

    Fig.6 shows the interfacial microstructure under different GNSs contents.When the GNSs content increased,Ti3Cu4and TiCu4were converted to TiCu in the brazing seam.The thickness of the TiC layer near C/C composite decreased while TiC particles were formed in the brazing seam(in Fig.6(a)–(d))because of the reaction between Ti and GNSs.Meanwhile,the thickness of the Ti-Cu reaction layer adjacent to TC4 alloy decreased.This may be attributed to the fact thatflaky GNSs hindered the diffusion of elements to the TC4 side.As adding 0.5–0.8wt%GNSs,the joining performance of brazed joints deteriorated because of the poorer wettability of AgCuTiGon the C/C composite surface.Combined with the prior wetting experiment results,owing to the poorer wettability of AgCuTiGfiller with more than 0.3wt%GNSs,defects were prone to occur on the interface adjacent to C/C composite.

    Fig.3 Microanalysis of droplet/C/C composite interface.

    Table 1 EDS results of spots marked in Fig.3(a1)–(a3)(at%).

    3.3.Effects of GNSs on the shear strength of C/C composite/TC4 brazed joints

    Fig.7 shows the effect of the GNSs content on the shear strength of C/C composite/AgCuTiG/TC4 joints brazed at 880°C for 10 min.It can be seen that the shear strength of brazed joints increased firstly and then decreased obviously with the increase of the GNSs content.The maximum shear strength of 23.3 MPa was obtained at 0.3wt%GNSs.The shear strength depended on the interfacial microstructure of brazed joints.Both the quantity and distribution of intermetallic compounds in the brazing seam,which were crucial factors in determining the shear strength of joints,varied with the addition of GNSs.As the GNSs content increased to 0.3wt%,the amount of block Ti-Cu intermetallic compounds decreased,and the formation of TiC particles by the reaction between GNSs and Ti in the filler could alleviate the residual stress.22With further increasing the GNSs content,owing to the impediment of GNSs,the diffusion of fewer Ti into the interlayer reduced the wetting and spreading of molten filler metal on the C/C composite surface.In addition,there existed a large mismatch of CTEs between the brazed seam and base materials at a high content of GNSs,which led to a strong residual stress in the brazed joints.Therefore,the brazed seam was prone to fracture under the condition of a high GNSs content.

    The fracture surface of C/C composite/TC4 brazed joints was investigated,and fracture morphologies after the shear test were examined by SEM,as shown in Fig.8.Different types of fracture modes were observed in the brazed joints at different GNSs contents.It indicated that fracture positions were closely related to the GNSs content and the directions of carbon fibers.When the GNSs content was low,the TiC layer could be a weak area of the joints due to the high residual stress caused by the mismatch of CTEs among AgCuTi,TiC and C/C composite.The shear strength of joints was relatively low,and crack mainly originated in the TiC layer.In the fracture process,the crack propagation was impeded by carbon fibers perpendicular to the brazing seam.However,due to the low bonding strength between carbon fibers parallel to the brazing seam and the C/C composite substrate,some carbon fibers were peeled off from C/C composite with the further increase of load.Thus,fracture occurred in C/C composite with carbon fibers parallel to the brazing seam while fracture appeared in the TiC layer with carbon fibers perpendicular to the brazing seam(Fig.8(a)and(b)).As adding GNSs to 0.3wt%,TiC particles were formed in situ,and GNSs reduced the CTE of braze alloy,thus relieving the residual stress of the bonding interface.A large amount of carbon fibers were pulled out,as shown in Fig.8(c).The pulling out of carbon fibers would consume energy,which led to the increase of the shear strength of joints.Fracture mainly occurred in C/C composite.The TiCu phase,Ag(s,s)and Cu(s,s)were observed at the fracture surface of joints with further increased GNSs.Fracture of joints occurred in the brazing seam,as shown in Fig.8(e).It indicated that more Ti in filler alloy would react with GNSs at a high GNSs content,resulting in weak bonding of joints.

    Fig.4 Interfacial microstructure of droplet/C/C composite with different GNSs contents.

    Fig.5 Interfacial microstructure of the C/C composite/AgCuTi/TC4 brazed joint.

    Table 2 EDS results of chemical compositions at each spot marked in Fig.5(at%).

    Fig.6 Interfacial microstructure of C/C composite/TC4 brazed joints with different GNSs contents.

    Fig.7 Effect of GNSs content on the shear strength of joints(T=880°C,t=10 min).

    4.Conclusions

    Sound brazing of C/C composite and TC4 alloy was realized using the GNSs reinforced AgCuTi composite filler in this study.The effects of the GNSs content on the wettability of AgCuTiGcomposite filler and the interfacial microstructure and mechanical properties of brazed joints were investigated.The following main conclusions were drawn:

    (1)The TiC layer was a key for filler alloy to wet C/C composite.GNSs,however,impeded the diffusion of Ti to the droplet/C/C composite interface.Therefore,the addition of GNSs reduced the wettability of filler on the C/C composite substrate.

    (2)With the increase of the GNSs content,the thickness of the reactive layer between the interface and base materials reduced,and the amount of block Ti-Cu compounds decreased.

    (3)The maximum shear strength of the joint brazed at 880°C for 10 min with 0.3wt%GNSs was 23.3 MPa.Further increasing the GNSs content deteriorated the shear strength of brazed joints.Fracture surface was observed for samples brazed with different GNSs contents.Fracture positions were related to the GNSs content and the directions of carbon fibers.Fracture paths extended from C/C composite to the brazing seam with the increase of GNSs.

    Acknowledgements

    We are grateful for thefinancial supports to this study from the National Natural Science Foundation of China–China(Nos.51505105 and 51775138),the Natural Science Foundation of Shandong Province–China(No.ZR2014EEQ001),and the International Science&Technology Cooperation Program of China–China(No.2015DFA50470).

    Fig.8 Fracture morphologies of C/C composite/TC4 joints with different GNSs contents.

    国产精品电影一区二区三区| 色综合站精品国产| 亚洲色图 男人天堂 中文字幕| 成人亚洲精品av一区二区| 亚洲av中文字字幕乱码综合| 欧美一区二区精品小视频在线| 99热只有精品国产| 成人av在线播放网站| 亚洲人成伊人成综合网2020| 久久精品国产综合久久久| 久久香蕉精品热| 一区福利在线观看| 亚洲欧美日韩卡通动漫| 国产亚洲欧美98| 一级毛片高清免费大全| 国产av在哪里看| 国产亚洲欧美在线一区二区| 精品一区二区三区视频在线 | 高清在线国产一区| 久久精品国产99精品国产亚洲性色| 一区福利在线观看| 国产私拍福利视频在线观看| 久久中文字幕人妻熟女| 亚洲av熟女| 1024手机看黄色片| 国产精品亚洲av一区麻豆| 99久久成人亚洲精品观看| 99国产精品99久久久久| 网址你懂的国产日韩在线| 午夜两性在线视频| 99国产极品粉嫩在线观看| 丰满的人妻完整版| 九九热线精品视视频播放| 最新中文字幕久久久久 | 国内精品美女久久久久久| 久久久久免费精品人妻一区二区| 欧美日韩亚洲国产一区二区在线观看| 高清毛片免费观看视频网站| 成年女人永久免费观看视频| 在线视频色国产色| 成人特级黄色片久久久久久久| 中文字幕高清在线视频| 国产 一区 欧美 日韩| 韩国av一区二区三区四区| 91九色精品人成在线观看| 搞女人的毛片| 国产伦精品一区二区三区四那| 亚洲午夜理论影院| 免费av不卡在线播放| 亚洲色图av天堂| 欧美一区二区精品小视频在线| 97碰自拍视频| 午夜影院日韩av| 久久精品aⅴ一区二区三区四区| 免费电影在线观看免费观看| 综合色av麻豆| 搡老妇女老女人老熟妇| 美女扒开内裤让男人捅视频| 熟女电影av网| 国产亚洲欧美在线一区二区| www国产在线视频色| 亚洲无线观看免费| 在线观看一区二区三区| 亚洲av熟女| 国产激情久久老熟女| 老熟妇乱子伦视频在线观看| 宅男免费午夜| www.www免费av| 国产人伦9x9x在线观看| 日韩欧美 国产精品| 哪里可以看免费的av片| 免费在线观看成人毛片| 又黄又粗又硬又大视频| 国产不卡一卡二| 日日干狠狠操夜夜爽| 欧美3d第一页| 国产精品99久久99久久久不卡| 色噜噜av男人的天堂激情| 亚洲aⅴ乱码一区二区在线播放| 亚洲av电影不卡..在线观看| 99视频精品全部免费 在线 | 亚洲自偷自拍图片 自拍| 国产精品久久久av美女十八| 91久久精品国产一区二区成人 | 99精品在免费线老司机午夜| ponron亚洲| 欧美性猛交黑人性爽| 97超级碰碰碰精品色视频在线观看| 亚洲成av人片在线播放无| 亚洲真实伦在线观看| 在线观看美女被高潮喷水网站 | 五月玫瑰六月丁香| 黑人操中国人逼视频| 亚洲av片天天在线观看| 亚洲中文字幕日韩| 在线视频色国产色| 岛国视频午夜一区免费看| 18禁美女被吸乳视频| a在线观看视频网站| 美女扒开内裤让男人捅视频| 我的老师免费观看完整版| 亚洲精品粉嫩美女一区| 欧美中文日本在线观看视频| 国内精品一区二区在线观看| 久久久久久久久久黄片| 免费在线观看成人毛片| 免费av不卡在线播放| 久久中文看片网| 欧美乱妇无乱码| 可以在线观看毛片的网站| 大型黄色视频在线免费观看| 成人午夜高清在线视频| 亚洲在线观看片| 男人舔女人的私密视频| 欧美激情在线99| 丰满人妻熟妇乱又伦精品不卡| 欧美三级亚洲精品| 黄色视频,在线免费观看| 性欧美人与动物交配| 欧美激情久久久久久爽电影| 十八禁网站免费在线| 国产麻豆成人av免费视频| 精品久久久久久成人av| 日韩精品中文字幕看吧| 国产精品久久久人人做人人爽| 国产亚洲av嫩草精品影院| 成人欧美大片| 精品国产三级普通话版| 在线观看免费午夜福利视频| h日本视频在线播放| 国产蜜桃级精品一区二区三区| 午夜福利视频1000在线观看| 亚洲无线观看免费| 精品乱码久久久久久99久播| av片东京热男人的天堂| 九九在线视频观看精品| 免费看美女性在线毛片视频| 午夜成年电影在线免费观看| 悠悠久久av| 舔av片在线| 欧美日韩亚洲国产一区二区在线观看| 一进一出抽搐gif免费好疼| 亚洲av电影在线进入| 亚洲第一欧美日韩一区二区三区| 999久久久精品免费观看国产| 国产一区二区激情短视频| 99久久精品国产亚洲精品| 欧美精品啪啪一区二区三区| 国产午夜精品久久久久久| 最新在线观看一区二区三区| 黑人巨大精品欧美一区二区mp4| 亚洲av成人av| 国产视频内射| 一区二区三区激情视频| 黄频高清免费视频| 黄色丝袜av网址大全| 色哟哟哟哟哟哟| 成在线人永久免费视频| 日本一本二区三区精品| av中文乱码字幕在线| 亚洲aⅴ乱码一区二区在线播放| 两个人看的免费小视频| 搡老岳熟女国产| 成人无遮挡网站| 欧美最黄视频在线播放免费| 午夜a级毛片| 桃红色精品国产亚洲av| 天天一区二区日本电影三级| 床上黄色一级片| 欧美一级毛片孕妇| 手机成人av网站| 国产野战对白在线观看| 国产亚洲精品久久久com| 国产精品永久免费网站| 夜夜看夜夜爽夜夜摸| 露出奶头的视频| 欧美日韩亚洲国产一区二区在线观看| 男人舔奶头视频| 欧美zozozo另类| 天堂网av新在线| 亚洲美女黄片视频| 两性夫妻黄色片| 在线观看舔阴道视频| 国产主播在线观看一区二区| 99久久精品国产亚洲精品| 黑人巨大精品欧美一区二区mp4| 久久精品综合一区二区三区| 在线播放国产精品三级| 亚洲精品一区av在线观看| 国产精品久久视频播放| 亚洲av中文字字幕乱码综合| 宅男免费午夜| 午夜福利成人在线免费观看| 此物有八面人人有两片| 嫁个100分男人电影在线观看| 亚洲av片天天在线观看| 日本精品一区二区三区蜜桃| www.精华液| 国产爱豆传媒在线观看| 男人的好看免费观看在线视频| 中文资源天堂在线| 亚洲av成人av| 天堂影院成人在线观看| 午夜福利18| 亚洲五月婷婷丁香| 国产精品一区二区三区四区免费观看 | 免费看光身美女| 美女高潮喷水抽搐中文字幕| 人妻久久中文字幕网| 人妻夜夜爽99麻豆av| 狠狠狠狠99中文字幕| 亚洲在线观看片| 18禁黄网站禁片免费观看直播| 午夜精品在线福利| 亚洲色图av天堂| 琪琪午夜伦伦电影理论片6080| 色综合欧美亚洲国产小说| 我的老师免费观看完整版| 成人午夜高清在线视频| 国产熟女xx| 亚洲激情在线av| 日本黄色片子视频| 男人舔女人的私密视频| 香蕉国产在线看| 成人高潮视频无遮挡免费网站| 一二三四社区在线视频社区8| 久久久久国产一级毛片高清牌| 我的老师免费观看完整版| 亚洲aⅴ乱码一区二区在线播放| 国产伦精品一区二区三区四那| 久久精品国产亚洲av香蕉五月| 无人区码免费观看不卡| 国产99白浆流出| 欧美zozozo另类| 一级毛片高清免费大全| 亚洲熟妇中文字幕五十中出| 久久久久精品国产欧美久久久| 午夜福利在线在线| 可以在线观看的亚洲视频| 免费av不卡在线播放| 欧美性猛交╳xxx乱大交人| 最新美女视频免费是黄的| 亚洲国产精品sss在线观看| 麻豆国产av国片精品| 成年版毛片免费区| 在线观看美女被高潮喷水网站 | 日韩有码中文字幕| 欧美日韩黄片免| av视频在线观看入口| 国产伦精品一区二区三区四那| 黄色女人牲交| 亚洲avbb在线观看| 国产成人系列免费观看| 久久久久性生活片| 伊人久久大香线蕉亚洲五| 久久久久九九精品影院| 国产黄片美女视频| 欧美日韩乱码在线| netflix在线观看网站| 18禁国产床啪视频网站| 欧洲精品卡2卡3卡4卡5卡区| 美女免费视频网站| 97超级碰碰碰精品色视频在线观看| 国产极品精品免费视频能看的| 51午夜福利影视在线观看| 波多野结衣巨乳人妻| 1024香蕉在线观看| www.熟女人妻精品国产| 色噜噜av男人的天堂激情| 99热6这里只有精品| 成年女人看的毛片在线观看| 中国美女看黄片| 超碰成人久久| 少妇裸体淫交视频免费看高清| 国产精品野战在线观看| 长腿黑丝高跟| 日本一本二区三区精品| 黄片小视频在线播放| 美女扒开内裤让男人捅视频| 美女午夜性视频免费| 成人鲁丝片一二三区免费| 精品不卡国产一区二区三区| 国产精品久久久久久人妻精品电影| 亚洲国产欧美网| 亚洲av成人av| 高潮久久久久久久久久久不卡| 午夜a级毛片| 性欧美人与动物交配| 成人av一区二区三区在线看| 欧美成人一区二区免费高清观看 | 久久性视频一级片| 亚洲中文字幕日韩| 又大又爽又粗| av天堂中文字幕网| 老鸭窝网址在线观看| 欧美绝顶高潮抽搐喷水| 少妇裸体淫交视频免费看高清| 成人精品一区二区免费| 欧美性猛交黑人性爽| 99热精品在线国产| 国产精品一区二区三区四区久久| 国产又黄又爽又无遮挡在线| 欧美午夜高清在线| 国内久久婷婷六月综合欲色啪| 男人舔奶头视频| 最近在线观看免费完整版| 国产亚洲av高清不卡| 99国产精品一区二区蜜桃av| 婷婷亚洲欧美| 国产成人精品久久二区二区91| 91九色精品人成在线观看| 19禁男女啪啪无遮挡网站| 国产精品一区二区免费欧美| 深夜精品福利| 淫妇啪啪啪对白视频| 他把我摸到了高潮在线观看| 国产激情久久老熟女| 成人三级黄色视频| 婷婷丁香在线五月| 一a级毛片在线观看| 欧美3d第一页| 丁香欧美五月| 老司机午夜福利在线观看视频| 亚洲精品一区av在线观看| 狂野欧美白嫩少妇大欣赏| 亚洲一区二区三区色噜噜| 亚洲五月婷婷丁香| 欧美日韩黄片免| 桃红色精品国产亚洲av| 国产极品精品免费视频能看的| www.www免费av| 免费av不卡在线播放| 色播亚洲综合网| 日韩精品中文字幕看吧| 99久久无色码亚洲精品果冻| 国产精品一区二区精品视频观看| 欧美成人一区二区免费高清观看 | 亚洲人成电影免费在线| 国产精品综合久久久久久久免费| 欧美色视频一区免费| 国产午夜福利久久久久久| 一边摸一边抽搐一进一小说| 日本成人三级电影网站| 俺也久久电影网| 亚洲欧美精品综合一区二区三区| 亚洲精品久久国产高清桃花| 在线a可以看的网站| 亚洲国产欧美一区二区综合| 麻豆成人av在线观看| 国产精品久久视频播放| 亚洲国产高清在线一区二区三| 国产成人影院久久av| 黑人巨大精品欧美一区二区mp4| 久久精品91无色码中文字幕| 国产亚洲av高清不卡| 在线观看午夜福利视频| 国产极品精品免费视频能看的| 亚洲五月婷婷丁香| 黄色 视频免费看| 精品欧美国产一区二区三| 欧美日韩黄片免| 欧美成狂野欧美在线观看| 九九在线视频观看精品| 男人和女人高潮做爰伦理| 亚洲一区二区三区色噜噜| 亚洲色图 男人天堂 中文字幕| 999精品在线视频| 给我免费播放毛片高清在线观看| 99久久久亚洲精品蜜臀av| av女优亚洲男人天堂 | 成人鲁丝片一二三区免费| 亚洲成人精品中文字幕电影| 成熟少妇高潮喷水视频| 丰满的人妻完整版| 两个人看的免费小视频| 国产一区二区在线av高清观看| 国产欧美日韩精品一区二区| 国产一区二区三区在线臀色熟女| 国产伦一二天堂av在线观看| 精品免费久久久久久久清纯| 国产精品一区二区三区四区免费观看 | 午夜免费激情av| 亚洲中文字幕日韩| 99精品久久久久人妻精品| 精品电影一区二区在线| 久久久久性生活片| 18禁黄网站禁片免费观看直播| 成熟少妇高潮喷水视频| 在线永久观看黄色视频| 亚洲av成人精品一区久久| www.999成人在线观看| 免费观看精品视频网站| 噜噜噜噜噜久久久久久91| 欧美乱码精品一区二区三区| 亚洲av熟女| 国产精品99久久99久久久不卡| 麻豆av在线久日| 九九在线视频观看精品| 成人av在线播放网站| 成人国产一区最新在线观看| 国产69精品久久久久777片 | 免费观看精品视频网站| 亚洲av日韩精品久久久久久密| 欧美高清成人免费视频www| 久久中文字幕人妻熟女| 老熟妇乱子伦视频在线观看| 男人的好看免费观看在线视频| 国产一级毛片七仙女欲春2| 久久久色成人| 成人特级黄色片久久久久久久| 一个人观看的视频www高清免费观看 | av福利片在线观看| 久久久久久大精品| 黑人欧美特级aaaaaa片| 国产成人系列免费观看| 亚洲avbb在线观看| 99热只有精品国产| 99国产精品99久久久久| 制服丝袜大香蕉在线| 国产精品一区二区三区四区免费观看 | av女优亚洲男人天堂 | www.精华液| 国产91精品成人一区二区三区| 天堂网av新在线| 欧美性猛交黑人性爽| 欧美乱色亚洲激情| 色精品久久人妻99蜜桃| 悠悠久久av| 精品一区二区三区四区五区乱码| 精华霜和精华液先用哪个| 国产精品久久电影中文字幕| 黄片小视频在线播放| 日日夜夜操网爽| 最近视频中文字幕2019在线8| 熟妇人妻久久中文字幕3abv| 亚洲国产欧美一区二区综合| 色哟哟哟哟哟哟| 精品无人区乱码1区二区| 少妇人妻一区二区三区视频| 国产高清videossex| 美女高潮喷水抽搐中文字幕| 天堂av国产一区二区熟女人妻| 亚洲国产欧美人成| 国产熟女xx| av视频在线观看入口| 在线a可以看的网站| 1024手机看黄色片| 久久人人精品亚洲av| 欧美另类亚洲清纯唯美| 亚洲18禁久久av| 真人做人爱边吃奶动态| 两个人视频免费观看高清| 久久国产精品影院| 午夜精品久久久久久毛片777| 亚洲真实伦在线观看| 欧美另类亚洲清纯唯美| 99精品欧美一区二区三区四区| 亚洲av中文字字幕乱码综合| 床上黄色一级片| 精品国产乱子伦一区二区三区| 久久99热这里只有精品18| 校园春色视频在线观看| 一级a爱片免费观看的视频| 一级黄色大片毛片| 久久久久久久精品吃奶| 色综合婷婷激情| 国产91精品成人一区二区三区| 亚洲欧美精品综合久久99| 村上凉子中文字幕在线| 美女 人体艺术 gogo| 12—13女人毛片做爰片一| 国产亚洲av嫩草精品影院| 18禁观看日本| 久久草成人影院| 宅男免费午夜| 亚洲午夜理论影院| 久久天躁狠狠躁夜夜2o2o| 免费在线观看影片大全网站| 国产69精品久久久久777片 | 少妇的逼水好多| а√天堂www在线а√下载| 熟女电影av网| x7x7x7水蜜桃| 日韩欧美精品v在线| 高清在线国产一区| 亚洲无线在线观看| 免费无遮挡裸体视频| 国产亚洲av嫩草精品影院| 国产精品影院久久| 国产精品永久免费网站| 久久久久久久午夜电影| 成年版毛片免费区| 国产真实乱freesex| 亚洲国产精品sss在线观看| 一本精品99久久精品77| 综合色av麻豆| 国产精品98久久久久久宅男小说| 亚洲国产色片| 精华霜和精华液先用哪个| 观看免费一级毛片| 一个人免费在线观看的高清视频| 亚洲欧美精品综合一区二区三区| 亚洲人与动物交配视频| 久久精品夜夜夜夜夜久久蜜豆| 国产探花在线观看一区二区| 日日干狠狠操夜夜爽| 亚洲中文字幕一区二区三区有码在线看 | 在线观看免费视频日本深夜| 国产精品美女特级片免费视频播放器 | 狂野欧美白嫩少妇大欣赏| 五月伊人婷婷丁香| 怎么达到女性高潮| 日本a在线网址| 老熟妇乱子伦视频在线观看| 久久精品91无色码中文字幕| 精品不卡国产一区二区三区| 久久久久九九精品影院| 中文亚洲av片在线观看爽| 又大又爽又粗| 九九在线视频观看精品| 日本 欧美在线| 国产精品98久久久久久宅男小说| av女优亚洲男人天堂 | 欧美一级a爱片免费观看看| 偷拍熟女少妇极品色| 九九在线视频观看精品| 色视频www国产| 亚洲,欧美精品.| 国产午夜精品论理片| 久久久久九九精品影院| 午夜福利18| 亚洲人成网站高清观看| 18禁美女被吸乳视频| 色哟哟哟哟哟哟| 91麻豆av在线| 亚洲精品国产精品久久久不卡| 757午夜福利合集在线观看| 成年人黄色毛片网站| 日韩欧美国产一区二区入口| 欧美中文日本在线观看视频| 亚洲专区中文字幕在线| 亚洲片人在线观看| 成人无遮挡网站| 999精品在线视频| 亚洲国产色片| 1000部很黄的大片| 热99re8久久精品国产| 男人舔奶头视频| 狂野欧美激情性xxxx| 国产精品久久久久久精品电影| 国产成人av激情在线播放| 麻豆国产97在线/欧美| 啦啦啦韩国在线观看视频| 90打野战视频偷拍视频| 亚洲国产欧美网| 老汉色av国产亚洲站长工具| 亚洲午夜理论影院| 久久久久久久午夜电影| 757午夜福利合集在线观看| 黄片大片在线免费观看| 精品人妻1区二区| 国产v大片淫在线免费观看| 宅男免费午夜| 精品一区二区三区av网在线观看| 国产精品日韩av在线免费观看| 亚洲成av人片在线播放无| 国产精品女同一区二区软件 | 日本黄色视频三级网站网址| 真人一进一出gif抽搐免费| 成人国产一区最新在线观看| 日本黄色片子视频| 18禁黄网站禁片免费观看直播| 成人三级做爰电影| 久久精品国产清高在天天线| 亚洲av成人精品一区久久| 19禁男女啪啪无遮挡网站| 好看av亚洲va欧美ⅴa在| 岛国在线免费视频观看| 日本成人三级电影网站| 免费观看的影片在线观看| 不卡一级毛片| 国产成人aa在线观看| 99国产极品粉嫩在线观看| www国产在线视频色| 婷婷六月久久综合丁香| 国产高清三级在线| 国产黄a三级三级三级人| 国产免费男女视频| 日韩欧美免费精品| 亚洲专区国产一区二区| 久9热在线精品视频| 亚洲乱码一区二区免费版| 亚洲第一电影网av| 五月玫瑰六月丁香| 亚洲av中文字字幕乱码综合| av在线天堂中文字幕| 亚洲国产精品合色在线| 青草久久国产| 神马国产精品三级电影在线观看| www国产在线视频色| 精品国产美女av久久久久小说| 脱女人内裤的视频| 淫秽高清视频在线观看| 又黄又爽又免费观看的视频| 日本一二三区视频观看| 精品电影一区二区在线| 亚洲精品456在线播放app | cao死你这个sao货| 国产一级毛片七仙女欲春2| 精品无人区乱码1区二区| 一级a爱片免费观看的视频| 日韩欧美在线二视频| 免费电影在线观看免费观看| 欧美日本视频| a级毛片在线看网站|